Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled

Category Polymer , Thermoplastic , Polyester, TP , Polybutylene Terephthalate (PBT) , Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled". Specific grades with glass content between 25% and 34% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.14 - 1.97 g/cc
0.0412 - 0.0712 lb/in³
Average value: 1.56 g/cc Grade Count:324
1.29 - 1.49 g/cc

@Temperature 250 - 250 °C
0.0466 - 0.0538 lb/in³

@Temperature 482 - 482 °F
Average value: 1.40 g/cc Grade Count:6
Filler Content 25.0 - 30.0 %
25.0 - 30.0 %
Average value: 29.8 % Grade Count:51
Water Absorption 0.0200 - 0.500 %
0.0200 - 0.500 %
Average value: 0.215 % Grade Count:100
Moisture Absorption at Equilibrium 0.0300 - 0.200 %
0.0300 - 0.200 %
Average value: 0.134 % Grade Count:121
Water Absorption at Saturation 0.0600 - 0.700 %
0.0600 - 0.700 %
Average value: 0.383 % Grade Count:19
Viscosity 230000 - 230000 cP

@Temperature 250 - 250 °C
230000 - 230000 cP

@Temperature 482 - 482 °F
Average value: 230000 cP Grade Count:2
230000 - 230000 cP

@Shear Rate 1000 - 1000 1/s
230000 - 230000 cP

@Shear Rate 1000 - 1000 1/s
Average value: 230000 cP Grade Count:2
Viscosity Test 62.0 - 111 cm³/g
62.0 - 111 cm³/g
Average value: 88.6 cm³/g Grade Count:31
Maximum Moisture Content 0.0200
0.0200
Average value: 0.0200 Grade Count:12
Linear Mold Shrinkage 0.000 - 0.0200 cm/cm
0.000 - 0.0200 in/in
Average value: 0.00468 cm/cm Grade Count:268
Linear Mold Shrinkage, Transverse 0.00100 - 0.0210 cm/cm
0.00100 - 0.0210 in/in
Average value: 0.00968 cm/cm Grade Count:124
Melt Flow 1.00 - 63.0 g/10 min
1.00 - 63.0 g/10 min
Average value: 19.0 g/10 min Grade Count:110
Spiral Flow 33.0 - 41.0 cm
13.0 - 16.1 in
Average value: 36.3 cm Grade Count:3
Ash 28.0 - 34.0 %
28.0 - 34.0 %
Average value: 30.4 % Grade Count:5
Mechanical Properties Metric English Comments
Hardness, Rockwell M 71.0 - 112
71.0 - 112
Average value: 89.2 Grade Count:33
Hardness, Rockwell R 90.0 - 122
90.0 - 122
Average value: 116 Grade Count:30
Hardness, Shore D 79.0 - 85.0
79.0 - 85.0
Average value: 82.0 Grade Count:7
Ball Indentation Hardness 105 - 230 MPa
15200 - 33400 psi
Average value: 185 MPa Grade Count:11
Tensile Strength, Ultimate 20.0 - 186 MPa
2900 - 27000 psi
Average value: 121 MPa Grade Count:263
15.0 - 195 MPa

@Temperature -40.0 - 150 °C
2180 - 28300 psi

@Temperature -40.0 - 302 °F
Average value: 93.9 MPa Grade Count:11
40.0 - 200 MPa

@Temperature -40.0 - 140 °C
5800 - 29000 psi

@Temperature -40.0 - 284 °F
Average value: 93.9 MPa Grade Count:1
40.0 - 200 MPa

@Strain 0.500 - 5.00 %
5800 - 29000 psi

@Strain 0.500 - 5.00 %
Average value: 93.9 MPa Grade Count:1
Tensile Strength, Yield 82.7 - 155 MPa
12000 - 22500 psi
Average value: 119 MPa Grade Count:81
Elongation at Break 1.00 - 130 %
1.00 - 130 %
Average value: 3.59 % Grade Count:274
1.90 - 6.30 %

@Temperature 0.000 - 150 °C
1.90 - 6.30 %

@Temperature 32.0 - 302 °F
Average value: 3.43 % Grade Count:9
Elongation at Yield 2.00 - 5.00 %
2.00 - 5.00 %
Average value: 2.97 % Grade Count:9
Modulus of Elasticity 0.824 - 15.0 GPa
119 - 2180 ksi
Average value: 9.44 GPa Grade Count:182
0.216 - 11.66 GPa

@Temperature -40.0 - 220 °C
31.3 - 1691 ksi

@Temperature -40.0 - 428 °F
Average value: 5.78 GPa Grade Count:14
Flexural Yield Strength 80.0 - 270 MPa
11600 - 39200 psi
Average value: 186 MPa Grade Count:236
115 - 120 MPa

@Temperature 90.0 - 90.0 °C
16700 - 17400 psi

@Temperature 194 - 194 °F
Average value: 118 MPa Grade Count:2
Flexural Modulus 0.00800 - 11.0 GPa
1.16 - 1600 ksi
Average value: 8.29 GPa Grade Count:234
4.80 - 5.50 GPa

@Temperature 90.0 - 90.0 °C
696 - 798 ksi

@Temperature 194 - 194 °F
Average value: 5.15 GPa Grade Count:2
Compressive Yield Strength 117 - 124 MPa
17000 - 18000 psi
Average value: 122 MPa Grade Count:6
Shear Modulus >= 0.380 GPa

@Temperature -100 - 200 °C
>= 55.1 ksi

@Temperature -148 - 392 °F
Average value: 1.30 GPa Grade Count:2
Izod Impact, Notched 0.150 - 2.19 J/cm
0.281 - 4.10 ft-lb/in
Average value: 0.904 J/cm Grade Count:146
0.96102 - 0.96102 J/cm

@Temperature -28.9 - -28.9 °C
1.8004 - 1.8004 ft-lb/in

@Temperature -20.0 - -20.0 °F
Average value: 0.961 J/cm Grade Count:1
Izod Impact, Unnotched 1.08 - 11.8 J/cm
2.02 - 22.0 ft-lb/in
Average value: 7.09 J/cm Grade Count:24
Izod Impact, Notched (ISO) 4.50 - 70.0 kJ/m²
2.14 - 33.3 ft-lb/in²
Average value: 13.0 kJ/m² Grade Count:88
6.00 - 32.0 kJ/m²

@Temperature -40.0 - 30.0 °C
2.86 - 15.2 ft-lb/in²

@Temperature -40.0 - 86.0 °F
Average value: 9.70 kJ/m² Grade Count:22
Izod Impact, Unnotched (ISO) 35.0 - 70.0 kJ/m²
16.7 - 33.3 ft-lb/in²
Average value: 54.0 kJ/m² Grade Count:39
30.0 - 60.0 kJ/m²

@Temperature -40.0 - -30.0 °C
14.3 - 28.6 ft-lb/in²

@Temperature -40.0 - -22.0 °F
Average value: 47.3 kJ/m² Grade Count:11
Charpy Impact Unnotched 0.850 - 50.0 J/cm²
4.05 - 238 ft-lb/in²
Average value: 5.67 J/cm² Grade Count:130
1.40 - 8.00 J/cm²

@Temperature -40.0 - 30.0 °C
6.66 - 38.1 ft-lb/in²

@Temperature -40.0 - 86.0 °F
Average value: 5.20 J/cm² Grade Count:84
Charpy Impact, Notched 0.210 - 7.50 J/cm²
0.999 - 35.7 ft-lb/in²
Average value: 0.984 J/cm² Grade Count:155
0.300 - 1.60 J/cm²

@Temperature -40.0 - 30.0 °C
1.43 - 7.61 ft-lb/in²

@Temperature -40.0 - 86.0 °F
Average value: 0.901 J/cm² Grade Count:89
Dart Drop, Total Energy 5.00 J
3.69 ft-lb
Average value: 5.00 J Grade Count:3
Puncture Energy 1.90 - 2.30 J
1.40 - 1.70 ft-lb
Average value: 2.22 J Grade Count:5
1.70 - 2.50 J

@Temperature -30.0 - -30.0 °C
1.25 - 1.84 ft-lb

@Temperature -22.0 - -22.0 °F
Average value: 2.10 J Grade Count:3
Tensile Creep Modulus, 1 hour 3600 - 11000 MPa
522000 - 1.60e+6 psi
Average value: 9640 MPa Grade Count:9
Tensile Creep Modulus, 1000 hours 2500 - 10000 MPa
363000 - 1.45e+6 psi
Average value: 7610 MPa Grade Count:14
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+8 - 2.00e+17 ohm-cm
1.00e+8 - 2.00e+17 ohm-cm
Average value: 1.62e+16 ohm-cm Grade Count:173
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved