Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Nylon 66, Unreinforced

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, Unreinforced
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Nylon 66, Unreinforced.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.02 - 2.70 g/cc
0.0368 - 0.0975 lb/in³
Average value: 1.14 g/cc Grade Count:328
0.980 - 0.980 g/cc

@Temperature 290 - 290 °C
0.0354 - 0.0354 lb/in³

@Temperature 554 - 554 °F
Average value: 0.980 g/cc Grade Count:1
Water Absorption 0.700 - 9.00 %
0.700 - 9.00 %
Average value: 4.39 % Grade Count:170
Moisture Absorption at Equilibrium 0.100 - 8.50 %
0.100 - 8.50 %
Average value: 2.42 % Grade Count:140
Water Absorption at Saturation 1.70 - 9.00 %
1.70 - 9.00 %
Average value: 7.91 % Grade Count:35
Viscosity 2.73 - 145 cP
2.73 - 145 cP
Average value: 51.2 cP Grade Count:8
Viscosity Test 115 - 330 cm³/g
115 - 330 cm³/g
Average value: 167 cm³/g Grade Count:16
Linear Mold Shrinkage 0.00100 - 0.0340 cm/cm
0.00100 - 0.0340 in/in
Average value: 0.0148 cm/cm Grade Count:214
Linear Mold Shrinkage, Transverse 0.00122 - 0.0250 cm/cm
0.00122 - 0.0250 in/in
Average value: 0.0164 cm/cm Grade Count:70
Melt Flow 2.00 - 148 g/10 min
2.00 - 148 g/10 min
Average value: 44.6 g/10 min Grade Count:34
Spiral Flow 104 - 105 cm
40.9 - 41.3 in
Average value: 104 cm Grade Count:4
Mechanical Properties Metric English Comments
Hardness, Rockwell M 55.0 - 90.0
55.0 - 90.0
Average value: 75.0 Grade Count:27
Hardness, Rockwell R 78.0 - 121
78.0 - 121
Average value: 114 Grade Count:66
Hardness, Shore D 77.0 - 88.0
77.0 - 88.0
Average value: 81.6 Grade Count:7
Ball Indentation Hardness 85.0 - 180 MPa
12300 - 26100 psi
Average value: 141 MPa Grade Count:11
Tensile Strength, Ultimate 15.0 - 100 MPa
2180 - 14500 psi
Average value: 71.3 MPa Grade Count:141
28.0 - 116 MPa

@Temperature -40.0 - 80.0 °C
4060 - 16800 psi

@Temperature -40.0 - 176 °F
Average value: 73.0 MPa Grade Count:2
Tensile Strength, Yield 30.0 - 98.0 MPa
4350 - 14200 psi
Average value: 72.2 MPa Grade Count:209
Elongation at Break 1.60 - 300 %
1.60 - 300 %
Average value: 54.0 % Grade Count:280
>= 100 %

@Temperature 60.0 - 150 °C
>= 100 %

@Temperature 140 - 302 °F
Average value: 100 % Grade Count:1
Elongation at Yield 3.40 - 100 %
3.40 - 100 %
Average value: 14.9 % Grade Count:153
Modulus of Elasticity 0.700 - 5.00 GPa
102 - 725 ksi
Average value: 2.51 GPa Grade Count:195
0.350 - 1.90 GPa

@Temperature 60.0 - 150 °C
50.8 - 276 ksi

@Temperature 140 - 302 °F
Average value: 0.850 GPa Grade Count:1
Flexural Yield Strength 11.0 - 140 MPa
1600 - 20300 psi
Average value: 93.6 MPa Grade Count:197
29.9922 - 140 MPa

@Temperature -40.0 - 90.0 °C
4350.01 - 20300 psi

@Temperature -40.0 - 194 °F
Average value: 71.0 MPa Grade Count:4
Flexural Modulus 0.750 - 7.60 GPa
109 - 1100 ksi
Average value: 2.49 GPa Grade Count:236
0.600 - 4.30 GPa

@Temperature -40.0 - 90.0 °C
87.0 - 624 ksi

@Temperature -40.0 - 194 °F
Average value: 1.92 GPa Grade Count:4
Compressive Yield Strength 7.00 - 100 MPa
1020 - 14500 psi
Average value: 46.3 MPa Grade Count:6
Poissons Ratio 0.380 - 0.450
0.380 - 0.450
Average value: 0.404 Grade Count:12
Shear Modulus 1.06 - 1.07 GPa
154 - 155 ksi
Average value: 1.07 GPa Grade Count:3
Shear Strength 50.0 - 65.0 MPa
7250 - 9430 psi
Average value: 58.0 MPa Grade Count:3
Izod Impact, Notched 0.300 - 8.54 J/cm
0.562 - 16.0 ft-lb/in
Average value: 1.04 J/cm Grade Count:119
0.350 - 0.480 J/cm

@Temperature -40.0 - -40.0 °C
0.656 - 0.899 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 0.427 J/cm Grade Count:5
0.490332 - 0.490332 J/cm

@Temperature 3.20 - 3.20 °C
0.918594 - 0.918594 ft-lb/in

@Temperature 37.8 - 37.8 °F
Average value: 0.427 J/cm Grade Count:1
0.490332 - 0.490332 J/cm

@Thickness 23.0 - 23.0 mm
0.918594 - 0.918594 ft-lb/in

@Thickness 0.906 - 0.906 in
Average value: 0.427 J/cm Grade Count:1
Izod Impact, Unnotched 0.534 J/cm - NB
1.00 ft-lb/in - NB
Average value: 9.53 J/cm Grade Count:9
Izod Impact, Notched (ISO) 3.15 kJ/m² - NB
1.50 ft-lb/in² - NB
Average value: 13.3 kJ/m² Grade Count:104
3.00 - 50.0 kJ/m²

@Temperature -40.0 - -20.0 °C
1.43 - 23.8 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 9.42 kJ/m² Grade Count:39
Izod Impact, Unnotched (ISO) 25.0 kJ/m² - NB
11.9 ft-lb/in² - NB
Average value: 67.3 kJ/m² Grade Count:9
300 kJ/m² - NB

@Temperature -30.0 - -30.0 °C
143 ft-lb/in² - NB

@Temperature -22.0 - -22.0 °F
Average value: 300 kJ/m² Grade Count:3
Charpy Impact Unnotched 2.00 J/cm² - NB
9.52 ft-lb/in² - NB
Average value: 9.76 J/cm² Grade Count:152
4.00 J/cm² - NB

@Temperature -40.0 - -20.0 °C
19.0 ft-lb/in² - NB

@Temperature -40.0 - -4.00 °F
Average value: 10.9 J/cm² Grade Count:98
Charpy Impact, Notched 0.100 - 1000 J/cm²
0.476 - 4760 ft-lb/in²
Average value: 1.21 J/cm² Grade Count:161
0.100 - 3.10 J/cm²

@Temperature -40.0 - -20.0 °C
0.476 - 14.8 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 0.690 J/cm² Grade Count:100
Puncture Energy 13.1 - 108 J
9.66 - 79.7 ft-lb
Average value: 36.1 J Grade Count:6
5.10 - 60.0 J

@Temperature -30.0 - -30.0 °C
3.76 - 44.3 ft-lb

@Temperature -22.0 - -22.0 °F
Average value: 25.2 J Grade Count:6
Coefficient of Friction 0.260 - 0.550
0.260 - 0.550
Average value: 0.369 Grade Count:6
Tensile Creep Modulus, 1 hour 1000 - 3400 MPa
145000 - 493000 psi
Average value: 2320 MPa Grade Count:14
Tensile Creep Modulus, 1000 hours 450 - 980 MPa
65300 - 142000 psi
Average value: 706 MPa Grade Count:14
Taber Abrasion, mg/1000 Cycles 4.00 - 8.00
4.00 - 8.00
Average value: 5.88 Grade Count:8
Electrical Properties Metric English Comments
Electrical Resistivity 4000 - 1.00e+19 ohm-cm
4000 - 1.00e+19 ohm-cm
Average value: 6.75e+16 ohm-cm Grade Count:139
Surface Resistance 350 - 2.50e+16 ohm
350 - 2.50e+16 ohm
Average value: 6.57e+14 ohm Grade Count:78
Dielectric Constant 1.90 - 15.0
1.90 - 15.0
Average value: 4.35 Grade Count:103
Dielectric Strength 11.8 - 120 kV/mm
300 - 3050 kV/in
Average value: 34.3 kV/mm Grade Count:109
Dissipation Factor 0.000200 - 0.320
0.000200 - 0.320
Average value: 0.0639 Grade Count:57
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved