Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Polyethylene Terephthalate (PET), Unreinforced

Category Polymer , Thermoplastic , Polyester, TP , Polyethylene Terephthalate (PET) , Polyethylene Terephthalate (PET), Unreinforced
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polyethylene Terephthalate (PET), Unreinforced.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polyethylene Terephthalate (PET), Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.25 - 1.45 g/cc
0.0452 - 0.0524 lb/in³
Average value: 1.37 g/cc Grade Count:99
1.10 - 1.20 g/cc

@Temperature 285 - 285 °C
0.0397 - 0.0434 lb/in³

@Temperature 545 - 545 °F
Average value: 1.19 g/cc Grade Count:27
Apparent Bulk Density 0.830 - 0.950 g/cc
0.0300 - 0.0343 lb/in³
Average value: 0.890 g/cc Grade Count:5
Water Absorption 0.0500 - 0.800 %
0.0500 - 0.800 %
Average value: 0.333 % Grade Count:22
Moisture Absorption at Equilibrium 0.200 - 0.300 %
0.200 - 0.300 %
Average value: 0.263 % Grade Count:19
Water Absorption at Saturation 0.400 - 0.500 %
0.400 - 0.500 %
Average value: 0.487 % Grade Count:12
Particle Size 2500 - 3500 µm
2500 - 3500 µm
Average value: 2800 µm Grade Count:47
Water Vapor Transmission 0.490 - 6.00 g/m²/day
0.0316 - 0.386 g/100 in²/day
Average value: 3.08 g/m²/day Grade Count:6
Oxygen Transmission 5.10 - 23.0 cc-mm/m²-24hr-atm
13.0 - 58.4 cc-mil/100 in²-24hr-atm
Average value: 11.1 cc-mm/m²-24hr-atm Grade Count:3
Oxygen Transmission Rate 2.00 - 20.0 cc/m²/day
0.129 - 1.29 cc/100 in²/day
Average value: 14.0 cc/m²/day Grade Count:3
Viscosity Test 62.0 - 86.0 cm³/g
62.0 - 86.0 cm³/g
Average value: 79.4 cm³/g Grade Count:12
Maximum Moisture Content 0.350 - 0.400
0.350 - 0.400
Average value: 0.360 Grade Count:5
Thickness 200 - 1200 microns
7.87 - 47.2 mil
Average value: 404 microns Grade Count:8
Linear Mold Shrinkage 0.00100 - 0.0200 cm/cm
0.00100 - 0.0200 in/in
Average value: 0.00525 cm/cm Grade Count:12
0.0100 - 0.0130 cm/cm

@Temperature 150 - 150 °C
0.0100 - 0.0130 in/in

@Temperature 302 - 302 °F
Average value: 0.0109 cm/cm Grade Count:17
0.0100 - 0.0130 cm/cm

@Time 900 - 900 sec
0.0100 - 0.0130 in/in

@Time 0.250 - 0.250 hour
Average value: 0.0109 cm/cm Grade Count:17
Linear Mold Shrinkage, Transverse 0.00200 - 0.0110 cm/cm
0.00200 - 0.0110 in/in
Average value: 0.00600 cm/cm Grade Count:3
0.00100 - 0.0100 cm/cm

@Temperature 150 - 150 °C
0.00100 - 0.0100 in/in

@Temperature 302 - 302 °F
Average value: 0.00500 cm/cm Grade Count:17
0.00100 - 0.0100 cm/cm

@Time 900 - 900 sec
0.00100 - 0.0100 in/in

@Time 0.250 - 0.250 hour
Average value: 0.00500 cm/cm Grade Count:17
Mechanical Properties Metric English Comments
Hardness, Rockwell M 80.0 - 96.0
80.0 - 96.0
Average value: 91.9 Grade Count:10
Hardness, Rockwell R 105 - 117
105 - 117
Average value: 110 Grade Count:11
Hardness, Shore D 79.0 - 81.0
79.0 - 81.0
Average value: 80.3 Grade Count:3
Ball Indentation Hardness 160 - 170 MPa
23200 - 24700 psi
Average value: 167 MPa Grade Count:6
Tensile Strength, Ultimate 22.0 - 90.0 MPa
3190 - 13100 psi
Average value: 45.3 MPa Grade Count:27
Film Tensile Strength at Yield, MD 55.0 - 260 MPa
7980 - 37700 psi
Average value: 176 MPa Grade Count:19
Film Tensile Strength at Yield, TD 53.0 - 265 MPa
7690 - 38400 psi
Average value: 206 MPa Grade Count:19
Tensile Strength, Yield 47.0 - 90.0 MPa
6820 - 13100 psi
Average value: 62.4 MPa Grade Count:26
Film Elongation at Break, MD 40.0 - 600 %
40.0 - 600 %
Average value: 192 % Grade Count:20
Film Elongation at Break, TD 100 - 600 %
100 - 600 %
Average value: 155 % Grade Count:19
Film Elongation at Yield, MD 4.00 - 6.00 %
4.00 - 6.00 %
Average value: 4.67 % Grade Count:3
Film Elongation at Yield, TD 4.00 - 6.00 %
4.00 - 6.00 %
Average value: 4.67 % Grade Count:3
Elongation at Break 4.00 - 600 %
4.00 - 600 %
Average value: 84.3 % Grade Count:36
Elongation at Yield 3.50 - 5.00 %
3.50 - 5.00 %
Average value: 4.09 % Grade Count:16
Modulus of Elasticity 1.83 - 5.20 GPa
265 - 754 ksi
Average value: 3.45 GPa Grade Count:43
Flexural Yield Strength 60.0 - 121 MPa
8700 - 17600 psi
Average value: 80.4 MPa Grade Count:20
Flexural Modulus 1.90 - 3.17 GPa
276 - 460 ksi
Average value: 2.41 GPa Grade Count:19
Compressive Yield Strength 20.0 - 103 MPa
2900 - 14900 psi
Average value: 59.2 MPa Grade Count:6
Izod Impact, Notched 0.139 - 100 J/cm
0.260 - 187 ft-lb/in
Average value: 0.629 J/cm Grade Count:16
0.270 - 0.630 J/cm

@Temperature -40.0 - -40.0 °C
0.506 - 1.18 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 0.395 J/cm Grade Count:11
Izod Impact, Unnotched 2.67 J/cm - NB
5.00 ft-lb/in - NB
Average value: 2.67 J/cm Grade Count:12
NB - NB

@Temperature -40.0 - -30.0 °C
NB - NB

@Temperature -40.0 - -22.0 °F
Grade Count:11
Izod Impact, Notched (ISO) 2.00 - 8.10 kJ/m²
0.952 - 3.85 ft-lb/in²
Average value: 4.73 kJ/m² Grade Count:10
3.10 - 4.20 kJ/m²

@Temperature -40.0 - -40.0 °C
1.48 - 2.00 ft-lb/in²

@Temperature -40.0 - -40.0 °F
Average value: 3.73 kJ/m² Grade Count:6
Izod Impact, Unnotched (ISO) NB
NB
Grade Count:3
160 - 181 kJ/m²

@Temperature -40.0 - -40.0 °C
76.1 - 86.1 ft-lb/in²

@Temperature -40.0 - -40.0 °F
Average value: 170 kJ/m² Grade Count:3
Charpy Impact Unnotched 3.00 J/cm² - NB
14.3 ft-lb/in² - NB
Average value: 5.04 J/cm² Grade Count:15
NB - NB

@Temperature -30.0 - -30.0 °C
NB - NB

@Temperature -22.0 - -22.0 °F
Grade Count:4
Charpy Impact, Notched 0.200 - 1.40 J/cm²
0.952 - 6.66 ft-lb/in²
Average value: 0.514 J/cm² Grade Count:19
0.270 - 0.500 J/cm²

@Temperature -30.0 - -30.0 °C
1.28 - 2.38 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 0.345 J/cm² Grade Count:4
Puncture Energy 12.0 - 41.0 J
8.85 - 30.2 ft-lb
Average value: 25.7 J Grade Count:8
13.0 - 39.0 J

@Temperature -40.0 - -40.0 °C
9.59 - 28.8 ft-lb

@Temperature -40.0 - -40.0 °F
Average value: 7.77 J Grade Count:4
0.800 - 24.0 J

@Temperature -40.0 - -40.0 °C
0.590 - 17.7 ft-lb

@Temperature -40.0 - -40.0 °F
Average value: 7.77 J Grade Count:4
0.800 - 24.0 J

@Thickness 2.50 - 3.20 mm
0.590 - 17.7 ft-lb

@Thickness 0.0984 - 0.126 in
Average value: 7.77 J Grade Count:4
Coefficient of Friction 0.180 - 0.300
0.180 - 0.300
Average value: 0.239 Grade Count:7
Coefficient of Friction, Static 0.190 - 0.400
0.190 - 0.400
Average value: 0.372 Grade Count:15
Chemical Properties Metric English Comments
Acetaldehyde 0.100 - 3.00 ppm
0.100 - 3.00 ppm
Average value: 1.23 ppm Grade Count:20
Users viewing this material also viewed the following: