Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Polyphenylene Sulfide (PPS), Unreinforced, Extruded

Category Polymer , Thermoplastic , Polyphenylene Sulfide (PPS) , Polyphenylene Sulfide (PPS), Unreinforced, Extruded
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polyphenylene Sulfide (PPS), Unreinforced, Extruded.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polyphenylene Sulfide (PPS), Unreinforced, Extruded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.34 - 1.65 g/cc
0.0484 - 0.0596 lb/in³
Average value: 1.40 g/cc Grade Count:18
Water Absorption 0.0100 - 0.0500 %
0.0100 - 0.0500 %
Average value: 0.0386 % Grade Count:7
Water Absorption at Saturation 0.0100 - 0.200 %
0.0100 - 0.200 %
Average value: 0.0575 % Grade Count:12
Linear Mold Shrinkage 0.00300 - 0.00900 cm/cm
0.00300 - 0.00900 in/in
Average value: 0.00600 cm/cm Grade Count:3
Melt Flow 45.0 - 170 g/10 min
45.0 - 170 g/10 min
Average value: 105 g/10 min Grade Count:6
Mechanical Properties Metric English Comments
Hardness, Rockwell M 82.0 - 100
82.0 - 100
Average value: 90.2 Grade Count:5
Hardness, Shore D 82.0 - 85.0
82.0 - 85.0
Average value: 83.7 Grade Count:3
Ball Indentation Hardness 160 - 205 MPa
23200 - 29700 psi
Average value: 185 MPa Grade Count:3
Tensile Strength, Ultimate 50.0 - 359 MPa
7250 - 52000 psi
Average value: 104 MPa Grade Count:18
Elongation at Break 2.00 - 40.0 %
2.00 - 40.0 %
Average value: 13.9 % Grade Count:19
Elongation at Yield 0.500 - 10.0 %
0.500 - 10.0 %
Average value: 4.32 % Grade Count:8
Modulus of Elasticity 3.20 - 14.0 GPa
464 - 2030 ksi
Average value: 5.74 GPa Grade Count:13
Flexural Yield Strength 72.0 - 155 MPa
10400 - 22500 psi
Average value: 114 MPa Grade Count:12
Flexural Modulus 3.20 - 12.0 GPa
464 - 1740 ksi
Average value: 5.51 GPa Grade Count:12
Compressive Yield Strength 33.0 - 148 MPa
4790 - 21500 psi
Average value: 87.0 MPa Grade Count:4
Izod Impact, Notched 0.320 - 2.51 J/cm
0.600 - 4.70 ft-lb/in
Average value: 0.928 J/cm Grade Count:5
Izod Impact, Notched (ISO) 2.00 - 4.00 kJ/m²
0.952 - 1.90 ft-lb/in²
Average value: 3.38 kJ/m² Grade Count:4
Charpy Impact Unnotched 0.400 - 1000 J/cm²
1.90 - 4760 ft-lb/in²
Average value: 0.975 J/cm² Grade Count:5
Charpy Impact, Notched 0.200 - 1000 J/cm²
0.952 - 4760 ft-lb/in²
Average value: 0.300 J/cm² Grade Count:3
Coefficient of Friction 0.200 - 0.600
0.200 - 0.600
Average value: 0.344 Grade Count:4
Limiting Pressure Velocity 0.105 - 0.430 MPa-m/sec
3000 - 12300 psi-ft/min
Average value: 0.278 MPa-m/sec Grade Count:3
Thermal Properties Metric English Comments
CTE, linear 50.0 - 60.0 µm/m-°C
27.8 - 33.3 µin/in-°F
Average value: 51.8 µm/m-°C Grade Count:11
120 - 120 µm/m-°C

@Temperature 100 - 200 °C
66.7 - 66.7 µin/in-°F

@Temperature 212 - 392 °F
Average value: 120 µm/m-°C Grade Count:2
Thermal Conductivity 0.288 - 22.0 W/m-K
2.00 - 153 BTU-in/hr-ft²-°F
Average value: 5.71 W/m-K Grade Count:10
Melting Point 280 - 285 °C
536 - 545 °F
Average value: 282 °C Grade Count:13
Maximum Service Temperature, Air 200 - 260 °C
392 - 500 °F
Average value: 227 °C Grade Count:9
Deflection Temperature at 1.8 MPa (264 psi) 95.0 - 260 °C
203 - 500 °F
Average value: 119 °C Grade Count:15
Glass Transition Temp, Tg 88.0 - 90.0 °C
190 - 194 °F
Average value: 89.6 °C Grade Count:5
Flammability, UL94 V-0
V-0
Grade Count:9
Oxygen Index 44.0 %
44.0 %
Average value: 44.0 % Grade Count:4
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+14 - 4.50e+16 ohm-cm
1.00e+14 - 4.50e+16 ohm-cm
Average value: 8.94e+15 ohm-cm Grade Count:12
Surface Resistance 1000 - 1.00e+16 ohm
1000 - 1.00e+16 ohm
Average value: 2.82e+15 ohm Grade Count:11
Insulation Resistance 1000 - 10000 ohm
1000 - 10000 ohm
Average value: 4000 ohm Grade Count:3
Dielectric Constant 2.70 - 3.30
2.70 - 3.30
Average value: 3.14 Grade Count:11
Dielectric Strength 18.0 - 24.0 kV/mm
457 - 610 kV/in
Average value: 22.5 kV/mm Grade Count:11
Dissipation Factor 0.00130 - 0.00300
0.00130 - 0.00300
Average value: 0.00203 Grade Count:9
Comparative Tracking Index 100 - 125 V
100 - 125 V
Average value: 117 V Grade Count:3
Processing Properties Metric English Comments
Processing Temperature 330 °C
626 °F
Average value: 330 °C Grade Count:3
Nozzle Temperature 320 - 340 °C
608 - 644 °F
Average value: 330 °C Grade Count:3
Melt Temperature 290 - 340 °C
554 - 644 °F
Average value: 317 °C Grade Count:6
Mold Temperature 150 - 180 °C
302 - 356 °F
Average value: 165 °C Grade Count:3
Drying Temperature 50.0 - 140 °C
122 - 284 °F
Average value: 102 °C Grade Count:5
Users viewing this material also viewed the following: