Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Polyphenylene Sulfide (PPS) with 30% Glass Fiber Filler

Category Polymer , Thermoplastic , Polyphenylene Sulfide (PPS) , Polyphenylene Sulfide (PPS) with 30% Glass Fiber Filler
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polyphenylene Sulfide (PPS) with 30% Glass Fiber Filler.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polyphenylene Sulfide (PPS) with 30% Glass Fiber Filler". Specific grades with glass content between 25% and 34% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.000809 - 1.69 g/cc
0.0000292 - 0.0611 lb/in³
Average value: 1.46 g/cc Grade Count:26
Filler Content 25.0 - 33.0 %
25.0 - 33.0 %
Average value: 29.8 % Grade Count:11
Water Absorption 0.0100 - 0.0500 %
0.0100 - 0.0500 %
Average value: 0.0245 % Grade Count:11
Linear Mold Shrinkage 0.000200 - 0.0100 cm/cm
0.000200 - 0.0100 in/in
Average value: 0.00308 cm/cm Grade Count:21
Linear Mold Shrinkage, Transverse 0.00500 - 0.00950 cm/cm
0.00500 - 0.00950 in/in
Average value: 0.00752 cm/cm Grade Count:11
Mechanical Properties Metric English Comments
Hardness, Rockwell M 86.0 - 100
86.0 - 100
Average value: 96.9 Grade Count:5
Hardness, Rockwell R 110 - 123
110 - 123
Average value: 119 Grade Count:4
Tensile Strength, Ultimate 33.1 - 203 MPa
4800 - 29400 psi
Average value: 140 MPa Grade Count:27
95.0 - 173.058 MPa

@Temperature -40.0 - 120 °C
13800 - 25100.0 psi

@Temperature -40.0 - 248 °F
Average value: 125 MPa Grade Count:2
Elongation at Break 0.500 - 4.00 %
0.500 - 4.00 %
Average value: 1.64 % Grade Count:26
1.30 - 1.30 %

@Temperature -40.0 - -40.0 °C
1.30 - 1.30 %

@Temperature -40.0 - -40.0 °F
Average value: 1.30 % Grade Count:1
Modulus of Elasticity 6.89 - 31.8 GPa
1000 - 4620 ksi
Average value: 13.8 GPa Grade Count:20
15.1685 - 15.1685 GPa

@Temperature -40.0 - -40.0 °C
2200.03 - 2200.03 ksi

@Temperature -40.0 - -40.0 °F
Average value: 15.2 GPa Grade Count:1
Flexural Yield Strength 53.1 - 339 MPa
7700 - 49200 psi
Average value: 208 MPa Grade Count:25
234.422 - 234.422 MPa

@Temperature -40.0 - -40.0 °C
34000.1 - 34000.1 psi

@Temperature -40.0 - -40.0 °F
Average value: 234 MPa Grade Count:1
Flexural Modulus 4.14 - 30.1 GPa
600 - 4360 ksi
Average value: 11.4 GPa Grade Count:26
6.50 - 12.1348 GPa

@Temperature -40.0 - 120 °C
943 - 1760.03 ksi

@Temperature -40.0 - 248 °F
Average value: 9.41 GPa Grade Count:2
Izod Impact, Notched 0.267 - 3.15 J/cm
0.500 - 5.90 ft-lb/in
Average value: 0.921 J/cm Grade Count:20
0.750 - 3.2034 J/cm

@Temperature -40.0 - -20.0 °C
1.41 - 6.0013 ft-lb/in

@Temperature -40.0 - -4.00 °F
Average value: 1.57 J/cm Grade Count:2
Izod Impact, Unnotched 2.14 - 6.90 J/cm
4.00 - 12.9 ft-lb/in
Average value: 4.31 J/cm Grade Count:14
Izod Impact, Notched (ISO) 9.00 - 30.0 kJ/m²
4.28 - 14.3 ft-lb/in²
Average value: 13.7 kJ/m² Grade Count:6
8.00 - 9.00 kJ/m²

@Temperature -30.0 - -30.0 °C
3.81 - 4.28 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 8.50 kJ/m² Grade Count:2
Izod Impact, Unnotched (ISO) 45.0 - 52.0 kJ/m²
21.4 - 24.7 ft-lb/in²
Average value: 48.3 kJ/m² Grade Count:3
Charpy Impact Unnotched 1.60 - 4.20 J/cm²
7.61 - 20.0 ft-lb/in²
Average value: 2.80 J/cm² Grade Count:4
1.60 - 4.20 J/cm²

@Temperature -40.0 - -20.0 °C
7.61 - 20.0 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 2.70 J/cm² Grade Count:3
Charpy Impact, Notched 0.600 - 1.45 J/cm²
2.86 - 6.90 ft-lb/in²
Average value: 0.950 J/cm² Grade Count:5
0.800 - 1.00 J/cm²

@Temperature -30.0 - -30.0 °C
3.81 - 4.76 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 0.900 J/cm² Grade Count:3
Thermal Properties Metric English Comments
CTE, linear 9.00 - 370 µm/m-°C
5.00 - 206 µin/in-°F
Average value: 66.6 µm/m-°C Grade Count:8
10.0 - 52.0 µm/m-°C

@Temperature 100 - 200 °C
5.56 - 28.9 µin/in-°F

@Temperature 212 - 392 °F
Average value: 31.0 µm/m-°C Grade Count:2
CTE, linear, Transverse to Flow 34.0 - 2980 µm/m-°C
18.9 - 1660 µin/in-°F
Average value: 473 µm/m-°C Grade Count:7
90.0 - 125 µm/m-°C

@Temperature 100 - 200 °C
50.0 - 69.4 µin/in-°F

@Temperature 212 - 392 °F
Average value: 108 µm/m-°C Grade Count:2
Melting Point 260 - 282 °C
500 - 540 °F
Average value: 277 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 200 - 280 °C
392 - 536 °F
Average value: 264 °C Grade Count:5
Deflection Temperature at 1.8 MPa (264 psi) 105 - 270 °C
221 - 518 °F
Average value: 255 °C Grade Count:23
Glass Transition Temp, Tg 90.0 °C
194 °F
Average value: 90.0 °C Grade Count:3
Flammability, UL94 V-0
V-0
Grade Count:17
Electrical Properties Metric English Comments
Electrical Resistivity 100 - 1.00e+18 ohm-cm
100 - 1.00e+18 ohm-cm
Average value: 7.19e+16 ohm-cm Grade Count:13
Surface Resistance 1000 - 1.00e+16 ohm
1000 - 1.00e+16 ohm
Average value: 3.07e+15 ohm Grade Count:8
Insulation Resistance 1.00e+11 - 1.00e+11 ohm

@Temperature 90.0 - 90.0 °C
1.00e+11 - 1.00e+11 ohm

@Temperature 194 - 194 °F
Average value: 1.00e+11 ohm Grade Count:1
Dielectric Constant 3.00 - 4.00
3.00 - 4.00
Average value: 3.57 Grade Count:7
Dielectric Strength 13.0 - 22.0 kV/mm
330 - 559 kV/in
Average value: 16.5 kV/mm Grade Count:6
Dissipation Factor 0.00100 - 0.00900
0.00100 - 0.00900
Average value: 0.00256 Grade Count:9
Arc Resistance 97.0 - 127 sec
97.0 - 127 sec
Average value: 120 sec Grade Count:6
Comparative Tracking Index 100 - 155 V
100 - 155 V
Average value: 141 V Grade Count:5
Processing Properties Metric English Comments
Processing Temperature 20.0 - 340 °C
68.0 - 644 °F
Average value: 207 °C Grade Count:9
Die Temperature 290 - 345 °C
554 - 653 °F
Average value: 318 °C Grade Count:7
Melt Temperature 20.0 - 345 °C
68.0 - 653 °F
Average value: 292 °C Grade Count:19
Mold Temperature 130 - 177 °C
266 - 350 °F
Average value: 151 °C Grade Count:17
Drying Temperature 110 - 150 °C
230 - 302 °F
Average value: 140 °C Grade Count:19
Moisture Content 0.0200 - 0.0400 %
0.0200 - 0.0400 %
Average value: 0.0314 % Grade Count:14
Injection Pressure 50.0 - 103 MPa
7250 - 15000 psi
Average value: 82.5 MPa Grade Count:15