Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled

Category Polymer , Thermoplastic , Liquid Crystal Polymer (LCP) , Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled". Specific grades with glass content between 25% and 34% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.36 - 1.69 g/cc
0.0491 - 0.0611 lb/in³
Average value: 1.61 g/cc Grade Count:54
Filler Content 30.0 %
30.0 %
Average value: 30.0 % Grade Count:13
Water Absorption 0.0200 - 1.30 %
0.0200 - 1.30 %
Average value: 0.214 % Grade Count:7
Moisture Absorption at Equilibrium 0.00200 - 0.0600 %
0.00200 - 0.0600 %
Average value: 0.0336 % Grade Count:9
Linear Mold Shrinkage -0.00100 - 0.00400 cm/cm
-0.00100 - 0.00400 in/in
Average value: 0.000879 cm/cm Grade Count:42
Linear Mold Shrinkage, Transverse 0.00100 - 0.00900 cm/cm
0.00100 - 0.00900 in/in
Average value: 0.00546 cm/cm Grade Count:35
Mechanical Properties Metric English Comments
Hardness, Rockwell M 40.0 - 100
40.0 - 100
Average value: 70.8 Grade Count:19
Hardness, Rockwell R 105 - 118
105 - 118
Average value: 109 Grade Count:6
Tensile Strength, Ultimate 26.6 - 211 MPa
3860 - 30600 psi
Average value: 144 MPa Grade Count:52
14.0 - 250 MPa

@Temperature -40.0 - 250 °C
2030 - 36300 psi

@Temperature -40.0 - 482 °F
Average value: 83.4 MPa Grade Count:3
14.0 - 250 MPa

@Thickness 0.800 - 3.17 mm
2030 - 36300 psi

@Thickness 0.0315 - 0.125 in
Average value: 83.4 MPa Grade Count:3
6.97 - 193.7 MPa

@Strain 0.0600 - 2.19 %
1010 - 28090 psi

@Strain 0.0600 - 2.19 %
Average value: 83.4 MPa Grade Count:1
6.97 - 193.7 MPa

@Temperature -40.0 - 200 °C
1010 - 28090 psi

@Temperature -40.0 - 392 °F
Average value: 83.4 MPa Grade Count:1
Tensile Strength, Yield 100 - 175 MPa
14500 - 25400 psi
Average value: 144 MPa Grade Count:4
Elongation at Break 0.700 - 6.20 %
0.700 - 6.20 %
Average value: 2.25 % Grade Count:52
0.800 - 1.40 %

@Temperature -40.0 - 250 °C
0.800 - 1.40 %

@Temperature -40.0 - 482 °F
Average value: 1.14 % Grade Count:1
0.800 - 1.40 %

@Thickness 1.60 - 1.60 mm
0.800 - 1.40 %

@Thickness 0.0630 - 0.0630 in
Average value: 1.14 % Grade Count:1
Modulus of Elasticity 5.50 - 31.8 GPa
798 - 4610 ksi
Average value: 14.3 GPa Grade Count:46
3.40 - 29.0 GPa

@Temperature -40.0 - 250 °C
493 - 4210 ksi

@Temperature -40.0 - 482 °F
Average value: 12.3 GPa Grade Count:3
3.40 - 29.0 GPa

@Thickness 1.60 - 3.17 mm
493 - 4210 ksi

@Thickness 0.0630 - 0.125 in
Average value: 12.3 GPa Grade Count:3
Flexural Yield Strength 124 - 300 MPa
18000 - 43500 psi
Average value: 197 MPa Grade Count:47
17.0 - 340 MPa

@Temperature -40.0 - 250 °C
2470 - 49300 psi

@Temperature -40.0 - 482 °F
Average value: 105 MPa Grade Count:3
17.0 - 340 MPa

@Thickness 0.800 - 3.17 mm
2470 - 49300 psi

@Thickness 0.0315 - 0.125 in
Average value: 105 MPa Grade Count:3
Flexural Modulus 6.60 - 26.0 GPa
957 - 3770 ksi
Average value: 13.7 GPa Grade Count:52
2.80 - 25.0 GPa

@Temperature -40.0 - 250 °C
406 - 3630 ksi

@Temperature -40.0 - 482 °F
Average value: 9.10 GPa Grade Count:3
2.80 - 25.0 GPa

@Thickness 0.800 - 3.17 mm
406 - 3630 ksi

@Thickness 0.0315 - 0.125 in
Average value: 9.10 GPa Grade Count:3
Compressive Yield Strength 38.0 - 204 MPa
5510 - 29600 psi
Average value: 107 MPa Grade Count:21
Compressive Modulus 6.00 - 33.0 GPa
870 - 4790 ksi
Average value: 16.8 GPa Grade Count:15
Shear Strength 51.0 - 68.0 MPa
7400 - 9860 psi
Average value: 58.2 MPa Grade Count:3
Izod Impact, Notched 0.167 - 4.00 J/cm
0.312 - 7.49 ft-lb/in
Average value: 1.63 J/cm Grade Count:17
1.10 - 4.90 J/cm

@Temperature -40.0 - -40.0 °C
2.06 - 9.18 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 2.67 J/cm Grade Count:3
1.10 - 4.90 J/cm

@Thickness 0.800 - 3.17 mm
2.06 - 9.18 ft-lb/in

@Thickness 0.0315 - 0.125 in
Average value: 2.67 J/cm Grade Count:3
Izod Impact, Unnotched 3.47 J/cm - NB
6.50 ft-lb/in - NB
Average value: 6.24 J/cm Grade Count:9
5.55 - 475 J/cm

@Temperature -40.0 - -40.0 °C
10.4 - 890 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 294 J/cm Grade Count:3
5.55 - 475 J/cm

@Thickness 0.800 - 3.17 mm
10.4 - 890 ft-lb/in

@Thickness 0.0315 - 0.125 in
Average value: 294 J/cm Grade Count:3
Izod Impact, Notched (ISO) 4.00 - 67.0 kJ/m²
1.90 - 31.9 ft-lb/in²
Average value: 22.5 kJ/m² Grade Count:30
20.0 - 20.0 kJ/m²

@Temperature -40.0 - -40.0 °C
9.52 - 9.52 ft-lb/in²

@Temperature -40.0 - -40.0 °F
Average value: 20.0 kJ/m² Grade Count:1
Izod Impact, Unnotched (ISO) 15.0 - 56.6 kJ/m²
7.14 - 26.9 ft-lb/in²
Average value: 34.8 kJ/m² Grade Count:7
30.0 - 30.0 kJ/m²

@Temperature -30.0 - -30.0 °C
14.3 - 14.3 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 30.0 kJ/m² Grade Count:1
Charpy Impact Unnotched 0.600 - 8.60 J/cm²
2.86 - 40.9 ft-lb/in²
Average value: 3.69 J/cm² Grade Count:28
2.20 - 3.00 J/cm²

@Temperature -30.0 - 30.0 °C
10.5 - 14.3 ft-lb/in²

@Temperature -22.0 - 86.0 °F
Average value: 2.52 J/cm² Grade Count:6
Charpy Impact, Notched 0.500 - 4.30 J/cm²
2.38 - 20.5 ft-lb/in²
Average value: 1.99 J/cm² Grade Count:34
1.50 - 3.00 J/cm²

@Temperature -30.0 - 30.0 °C
7.14 - 14.3 ft-lb/in²

@Temperature -22.0 - 86.0 °F
Average value: 2.29 J/cm² Grade Count:7
Tensile Creep Modulus, 1 hour 9800 - 19600 MPa
1.42e+6 - 2.84e+6 psi
Average value: 14000 MPa Grade Count:6
Tensile Creep Modulus, 1000 hours 7500 - 15800 MPa
1.09e+6 - 2.29e+6 psi
Average value: 11800 MPa Grade Count:6
Electrical Properties Metric English Comments
Electrical Resistivity 100 - 1.00e+17 ohm-cm
100 - 1.00e+17 ohm-cm
Average value: 5.11e+15 ohm-cm Grade Count:37
Surface Resistance 10.0 - 1.00e+17 ohm
10.0 - 1.00e+17 ohm
Average value: 6.89e+15 ohm Grade Count:37
Dielectric Constant 2.70 - 32.0
2.70 - 32.0
Average value: 4.72 Grade Count:32
4.10 - 5.00

@Temperature 100 - 250 °C
4.10 - 5.00

@Temperature 212 - 482 °F
Average value: 4.55 Grade Count:5
4.10 - 5.00

@Frequency 1000 - 1.00e+9 Hz
4.10 - 5.00

@Frequency 1000 - 1.00e+9 Hz
Average value: 4.55 Grade Count:5
Dielectric Strength 16.1 - 56.0 kV/mm
410 - 1420 kV/in
Average value: 33.4 kV/mm Grade Count:26