Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Acetal Copolymer, Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.14 - 2.23 g/cc
0.0412 - 0.0806 lb/in³
Average value: 1.42 g/cc Grade Count:376
1.43 - 1.43 g/cc

@Temperature 215 - 215 °C
0.0517 - 0.0517 lb/in³

@Temperature 419 - 419 °F
Average value: 1.43 g/cc Grade Count:1
Water Absorption 0.0500 - 7.90 %
0.0500 - 7.90 %
Average value: 0.623 % Grade Count:128
Moisture Absorption at Equilibrium 0.100 - 2.20 %
0.100 - 2.20 %
Average value: 0.261 % Grade Count:130
Water Absorption at Saturation 0.220 - 10.0 %
0.220 - 10.0 %
Average value: 1.20 % Grade Count:33
Maximum Moisture Content 0.100
0.100
Average value: 0.100 Grade Count:9
Linear Mold Shrinkage 0.00120 - 0.0400 cm/cm
0.00120 - 0.0400 in/in
Average value: 0.0207 cm/cm Grade Count:256
Linear Mold Shrinkage, Transverse 0.00210 - 0.0400 cm/cm
0.00210 - 0.0400 in/in
Average value: 0.0208 cm/cm Grade Count:102
Melt Flow 1.00 - 58.8 g/10 min
1.00 - 58.8 g/10 min
Average value: 15.7 g/10 min Grade Count:223
Mechanical Properties Metric English Comments
Hardness, Rockwell M 50.0 - 97.0
50.0 - 97.0
Average value: 81.1 Grade Count:77
Hardness, Rockwell R 69.0 - 121
69.0 - 121
Average value: 100 Grade Count:57
Hardness, Shore D 75.0 - 85.0
75.0 - 85.0
Average value: 80.4 Grade Count:12
Ball Indentation Hardness 30.0 - 179 MPa
4350 - 26000 psi
Average value: 134 MPa Grade Count:74
Tensile Strength, Ultimate 5.00 - 117 MPa
725 - 17000 psi
Average value: 53.3 MPa Grade Count:181
Tensile Strength, Yield 22.0 - 120 MPa
3190 - 17400 psi
Average value: 57.4 MPa Grade Count:244
25.0 - 93.0 MPa

@Temperature -40.0 - 120 °C
3630 - 13500 psi

@Temperature -40.0 - 248 °F
Average value: 46.5 MPa Grade Count:3
Elongation at Break 0.700 - 250 %
0.700 - 250 %
Average value: 34.8 % Grade Count:317
>= 100 %

@Temperature 60.0 - 90.0 °C
>= 100 %

@Temperature 140 - 194 °F
Average value: 100 % Grade Count:7
Elongation at Yield 1.10 - 29.0 %
1.10 - 29.0 %
Average value: 10.7 % Grade Count:123
5.80 - 10.0 %

@Temperature -40.0 - 80.0 °C
5.80 - 10.0 %

@Temperature -40.0 - 176 °F
Average value: 8.37 % Grade Count:2
Modulus of Elasticity 0.586 - 20.7 GPa
85.0 - 3000 ksi
Average value: 2.80 GPa Grade Count:238
0.500 - 1.90 GPa

@Temperature 60.0 - 90.0 °C
72.5 - 276 ksi

@Temperature 140 - 194 °F
Average value: 1.78 GPa Grade Count:8
2.41 - 2.81 GPa

@Temperature 30.0 - 120 °C
350 - 408 ksi

@Temperature 86.0 - 248 °F
Average value: 1.78 GPa Grade Count:1
2.41 - 2.81 GPa

@Thickness 1.50 - 4.00 mm
350 - 408 ksi

@Thickness 0.0591 - 0.157 in
Average value: 1.78 GPa Grade Count:1
Flexural Yield Strength 13.0 - 179 MPa
1890 - 26000 psi
Average value: 78.4 MPa Grade Count:230
Flexural Modulus 0.276 - 17.3 GPa
40.0 - 2510 ksi
Average value: 2.63 GPa Grade Count:256
Compressive Yield Strength 14.0 - 110 MPa
2030 - 16000 psi
Average value: 60.5 MPa Grade Count:20
Compressive Modulus 1.21 - 2.76 GPa
175 - 400 ksi
Average value: 2.30 GPa Grade Count:6
Poissons Ratio 0.350 - 0.430
0.350 - 0.430
Average value: 0.363 Grade Count:6
Shear Strength 40.0 - 55.2 MPa
5800 - 8000 psi
Average value: 51.9 MPa Grade Count:18
Izod Impact, Notched 0.0500 J/cm - NB
0.0937 ft-lb/in - NB
Average value: 1.04 J/cm Grade Count:174
0.300 - 1.00 J/cm

@Temperature -40.0 - -29.0 °C
0.562 - 1.87 ft-lb/in

@Temperature -40.0 - -20.2 °F
Average value: 0.565 J/cm Grade Count:9
Izod Impact, Unnotched 0.480 J/cm - NB
0.899 ft-lb/in - NB
Average value: 7.02 J/cm Grade Count:48
Izod Impact, Notched (ISO) 2.50 - 47.0 kJ/m²
1.19 - 22.4 ft-lb/in²
Average value: 8.19 kJ/m² Grade Count:104
5.00 - 7.00 kJ/m²

@Temperature -40.0 - -30.0 °C
2.38 - 3.33 ft-lb/in²

@Temperature -40.0 - -22.0 °F
Average value: 5.88 kJ/m² Grade Count:16
Izod Impact, Unnotched (ISO) 15.0 kJ/m² - NB
7.14 ft-lb/in² - NB
Average value: 129 kJ/m² Grade Count:51
Charpy Impact Unnotched 2.40 J/cm² - NB
11.4 ft-lb/in² - NB
Average value: 16.1 J/cm² Grade Count:94
2.00 J/cm² - NB

@Temperature -40.0 - -20.0 °C
9.52 ft-lb/in² - NB

@Temperature -40.0 - -4.00 °F
Average value: 17.6 J/cm² Grade Count:52
Charpy Impact, Notched 0.300 - 1000 J/cm²
1.43 - 4760 ft-lb/in²
Average value: 0.664 J/cm² Grade Count:161
0.250 J/cm² - NB

@Temperature -30.0 - -20.0 °C
1.19 ft-lb/in² - NB

@Temperature -22.0 - -4.00 °F
Average value: 0.568 J/cm² Grade Count:50
Gardner Impact 22.6 - 22.6 J
16.7 - 16.7 ft-lb
Average value: 22.6 J Grade Count:5
Tensile Impact Strength 110 - 280 kJ/m²
52.3 - 133 ft-lb/in²
Average value: 167 kJ/m² Grade Count:5
Dart Drop, Total Energy 3.00 - 29.0 J
2.21 - 21.4 ft-lb
Average value: 7.04 J Grade Count:27
Falling Dart Impact 22.6 - 32.1 J
16.7 - 23.7 ft-lb
Average value: 27.8 J Grade Count:3
Coefficient of Friction 0.0980 - 0.560
0.0980 - 0.560
Average value: 0.247 Grade Count:71
0.200 - 0.200

@Temperature 60.0 - 60.0 °C
0.200 - 0.200

@Temperature 140 - 140 °F
Average value: 0.200 Grade Count:1
Coefficient of Friction, Static 0.110 - 0.440
0.110 - 0.440
Average value: 0.175 Grade Count:48
Tensile Creep Modulus, 1 hour 1800 - 2500 MPa
261000 - 363000 psi
Average value: 2280 MPa Grade Count:11
Tensile Creep Modulus, 1000 hours 400 - 1450 MPa
58000 - 210000 psi
Average value: 1160 MPa Grade Count:40
K (wear) Factor 16.1 - 806 x 10-8 mm³/N-M
8.00 - 400 x 10-10 in³-min/ft-lb-hr
Average value: 86.1 x 10<sup>-8</sup> mm³/N-M Grade Count:30
Limiting Pressure Velocity 0.0701 - 0.590 MPa-m/sec
2000 - 16800 psi-ft/min
Average value: 0.167 MPa-m/sec Grade Count:8
Taber Abrasion, mg/1000 Cycles 14.0
14.0
Average value: 14.0 Grade Count:18
Electrical Properties Metric English Comments
Electrical Resistivity 0.200 - 1.00e+16 ohm-cm
0.200 - 1.00e+16 ohm-cm
Average value: 1.73e+15 ohm-cm Grade Count:175
Surface Resistance 10.0 - 1.00e+16 ohm
10.0 - 1.00e+16 ohm
Average value: 3.03e+15 ohm Grade Count:184
Insulation Resistance 1.00e+11 - 1.00e+12 ohm
1.00e+11 - 1.00e+12 ohm
Average value: 4.60e+11 ohm Grade Count:5
Static Decay 0.00300 - 2.00 sec
0.00300 - 2.00 sec
Average value: 1.38 sec Grade Count:6
Dielectric Constant 3.40 - 5.00
3.40 - 5.00
Average value: 3.85 Grade Count:112