Overview of materials for Nylon 66, Aramid Fiber Filled

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, Aramid Fiber Filled
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Nylon 66, Aramid Fiber Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, Aramid Fiber Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.14 - 1.39 g/cc
0.0412 - 0.0502 lb/in³
Average value: 1.22 g/cc Grade Count:51
Filler Content 5.00 - 25.0 %
5.00 - 25.0 %
Average value: 15.0 % Grade Count:8
Water Absorption 0.500 - 6.80 %
0.500 - 6.80 %
Average value: 1.12 % Grade Count:26
Additive Loading 10.0 - 15.0 %
10.0 - 15.0 %
Average value: 11.4 % Grade Count:7
Linear Mold Shrinkage 0.00100 - 0.0300 cm/cm
0.00100 - 0.0300 in/in
Average value: 0.0118 cm/cm Grade Count:49
Linear Mold Shrinkage, Transverse 0.00500 - 0.0240 cm/cm
0.00500 - 0.0240 in/in
Average value: 0.0171 cm/cm Grade Count:8
Mechanical Properties Metric English Comments
Hardness, Rockwell R 100 - 120
100 - 120
Average value: 113 Grade Count:8
Tensile Strength, Ultimate 48.3 - 138 MPa
7000 - 20000 psi
Average value: 88.2 MPa Grade Count:45
Tensile Strength, Yield 81.4 - 110 MPa
11800 - 16000 psi
Average value: 94.0 MPa Grade Count:7
Elongation at Break 1.60 - 10.0 %
1.60 - 10.0 %
Average value: 5.59 % Grade Count:42
Elongation at Yield 3.50 - 8.40 %
3.50 - 8.40 %
Average value: 5.77 % Grade Count:10
Modulus of Elasticity 2.41 - 11.0 GPa
350 - 1600 ksi
Average value: 4.79 GPa Grade Count:42
Flexural Yield Strength 75.8 - 207 MPa
11000 - 30000 psi
Average value: 130 MPa Grade Count:47
Flexural Modulus 0.621 - 8.27 GPa
90.0 - 1200 ksi
Average value: 3.90 GPa Grade Count:47
Izod Impact, Notched 0.320 - 1.44 J/cm
0.599 - 2.70 ft-lb/in
Average value: 0.597 J/cm Grade Count:37
Izod Impact, Unnotched 2.14 - 11.2 J/cm
4.00 - 21.0 ft-lb/in
Average value: 5.46 J/cm Grade Count:29
Izod Impact, Notched (ISO) 4.00 - 5.80 kJ/m²
1.90 - 2.76 ft-lb/in²
Average value: 4.96 kJ/m² Grade Count:5
Izod Impact, Unnotched (ISO) 35.0 - 48.6 kJ/m²
16.7 - 23.1 ft-lb/in²
Average value: 39.4 kJ/m² Grade Count:4
Charpy Impact Unnotched 2.00 - 6.50 J/cm²
9.52 - 30.9 ft-lb/in²
Average value: 4.05 J/cm² Grade Count:12
Charpy Impact, Notched 0.200 - 1.50 J/cm²
0.952 - 7.14 ft-lb/in²
Average value: 0.533 J/cm² Grade Count:11
Coefficient of Friction 0.130 - 0.550
0.130 - 0.550
Average value: 0.244 Grade Count:10
Coefficient of Friction, Static 0.110 - 0.570
0.110 - 0.570
Average value: 0.273 Grade Count:12
K (wear) Factor 7.50 - 46.3 x 10-8 mm³/N-M
3.72 - 23.0 x 10-10 in³-min/ft-lb-hr
Average value: 27.7 x 10<sup>-8</sup> mm³/N-M Grade Count:5
Thermal Properties Metric English Comments
CTE, linear 28.8 - 67.0 µm/m-°C
16.0 - 37.2 µin/in-°F
Average value: 54.8 µm/m-°C Grade Count:10
CTE, linear, Transverse to Flow 75.0 - 97.0 µm/m-°C
41.7 - 53.9 µin/in-°F
Average value: 89.7 µm/m-°C Grade Count:3
Melting Point 255 - 265 °C
491 - 509 °F
Average value: 259 °C Grade Count:7
Maximum Service Temperature, Air 90.0 - 160 °C
194 - 320 °F
Average value: 134 °C Grade Count:10
Deflection Temperature at 0.46 MPa (66 psi) 232 - 255 °C
450 - 491 °F
Average value: 241 °C Grade Count:19
Deflection Temperature at 1.8 MPa (264 psi) 70.0 - 246 °C
158 - 475 °F
Average value: 171 °C Grade Count:44
Vicat Softening Point 240 - 260 °C
464 - 500 °F
Average value: 254 °C Grade Count:9
Flammability, UL94 HB
HB
Grade Count:25
Electrical Properties Metric English Comments
Electrical Resistivity 1e+05 - 1.00e+17 ohm-cm
1e+05 - 1.00e+17 ohm-cm
Average value: 5.92e+15 ohm-cm Grade Count:23
Surface Resistance 1.00e+13 - 1.00e+15 ohm
1.00e+13 - 1.00e+15 ohm
Average value: 1.08e+14 ohm Grade Count:11
Insulation Resistance 1.00e+12 ohm
1.00e+12 ohm
Average value: 1.00e+12 ohm Grade Count:9
Dielectric Strength 17.7 - 23.0 kV/mm
450 - 584 kV/in
Average value: 19.2 kV/mm Grade Count:5
Processing Properties Metric English Comments
Processing Temperature 80.0 - 300 °C
176 - 572 °F
Average value: 277 °C Grade Count:21
Nozzle Temperature 280 - 300 °C
536 - 572 °F
Average value: 290 °C Grade Count:9
Melt Temperature 70.0 - 315 °C
158 - 599 °F
Average value: 290 °C Grade Count:33
Mold Temperature 60.0 - 120 °C
140 - 248 °F
Average value: 90.6 °C Grade Count:43
Drying Temperature 70.0 - 105 °C
158 - 221 °F
Average value: 84.8 °C Grade Count:34
Moisture Content 0.150 - 0.250 %
0.150 - 0.250 %
Average value: 0.199 % Grade Count:23
Dew Point -17.8 °C
0.000 °F
Average value: -17.8 °C Grade Count:14
Injection Pressure 68.9 - 124 MPa
10000 - 18000 psi
Average value: 100 MPa Grade Count:24