Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, 40% Glass Fiber Filled". Specific grades with glass content between 35% and 44% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.20 - 1.72 g/cc
0.0434 - 0.0621 lb/in³
Average value: 1.45 g/cc Grade Count:331
1.24 - 1.29 g/cc

@Temperature 250 - 295 °C
0.0448 - 0.0466 lb/in³

@Temperature 482 - 563 °F
Average value: 1.26 g/cc Grade Count:7
Filler Content 30.0 - 46.0 %
30.0 - 46.0 %
Average value: 39.5 % Grade Count:67
Water Absorption 0.300 - 7.60 %
0.300 - 7.60 %
Average value: 2.02 % Grade Count:154
1.30 - 2.00 %

@Temperature 70.0 - 70.0 °C
1.30 - 2.00 %

@Temperature 158 - 158 °F
Average value: 1.74 % Grade Count:5
Moisture Absorption at Equilibrium 0.170 - 2.30 %
0.170 - 2.30 %
Average value: 1.45 % Grade Count:99
Water Absorption at Saturation 0.0200 - 8.00 %
0.0200 - 8.00 %
Average value: 4.70 % Grade Count:47
Additive Loading 35.0 - 40.0 %
35.0 - 40.0 %
Average value: 38.8 % Grade Count:4
Viscosity 20.0 - 300 cP

@Temperature 275 - 300 °C
20.0 - 300 cP

@Temperature 527 - 572 °F
Average value: 144 cP Grade Count:2
20.0 - 300 cP

@Shear Rate 10.0 - 1000 1/s
20.0 - 300 cP

@Shear Rate 10.0 - 1000 1/s
Average value: 144 cP Grade Count:2
Viscosity Test 140 - 150 cm³/g
140 - 150 cm³/g
Average value: 144 cm³/g Grade Count:9
Linear Mold Shrinkage 0.00000500 - 0.0250 cm/cm
0.00000500 - 0.0250 in/in
Average value: 0.00407 cm/cm Grade Count:262
Linear Mold Shrinkage, Transverse 0.0000300 - 0.105 cm/cm
0.0000300 - 0.105 in/in
Average value: 0.00822 cm/cm Grade Count:114
Melt Flow 1.00 - 56.4 g/10 min
1.00 - 56.4 g/10 min
Average value: 25.8 g/10 min Grade Count:30
Spiral Flow 66.0 - 664 cm
26.0 - 261 in
Average value: 129 cm Grade Count:11
Mechanical Properties Metric English Comments
Hardness, Rockwell L 108 - 115
108 - 115
Average value: 113 Grade Count:5
Hardness, Rockwell M 80.0 - 105
80.0 - 105
Average value: 95.7 Grade Count:27
Hardness, Rockwell R 111 - 125
111 - 125
Average value: 121 Grade Count:58
Hardness, Shore D 81.0 - 86.0
81.0 - 86.0
Average value: 83.2 Grade Count:4
Ball Indentation Hardness 130 - 310 MPa
18900 - 45000 psi
Average value: 254 MPa Grade Count:23
Tensile Strength, Ultimate 50.0 - 294 MPa
7250 - 42600 psi
Average value: 182 MPa Grade Count:253
45.0 - 269.585 MPa

@Temperature -40.0 - 150 °C
6530 - 39100.1 psi

@Temperature -40.0 - 302 °F
Average value: 101 MPa Grade Count:9
100 - 115 MPa

@Temperature 130 - 175 °C
14500 - 16700 psi

@Temperature 266 - 347 °F
Average value: 101 MPa Grade Count:5
100 - 115 MPa

@Time 1.80e+7 - 7.20e+7 sec
14500 - 16700 psi

@Time 5000 - 20000 hour
Average value: 101 MPa Grade Count:5
25.0 - 400 MPa

@Strain 1.00 - 10.0 %
3630 - 58000 psi

@Strain 1.00 - 10.0 %
Average value: 101 MPa Grade Count:5
25.0 - 400 MPa

@Temperature -40.0 - 200 °C
3630 - 58000 psi

@Temperature -40.0 - 392 °F
Average value: 101 MPa Grade Count:5
Tensile Strength, Yield 55.0 - 230 MPa
7980 - 33400 psi
Average value: 184 MPa Grade Count:94
Elongation at Break 1.00 - 35.0 %
1.00 - 35.0 %
Average value: 3.30 % Grade Count:303
2.00 - 5.60 %

@Temperature -40.0 - 150 °C
2.00 - 5.60 %

@Temperature -40.0 - 302 °F
Average value: 3.57 % Grade Count:8
Elongation at Yield 1.80 - 20.0 %
1.80 - 20.0 %
Average value: 4.23 % Grade Count:28
Modulus of Elasticity 1.30 - 30.9 GPa
189 - 4480 ksi
Average value: 11.1 GPa Grade Count:218
2.714 - 15.13 GPa

@Temperature -40.0 - 220 °C
393.6 - 2194 ksi

@Temperature -40.0 - 428 °F
Average value: 7.37 GPa Grade Count:15
Flexural Yield Strength 75.0 - 455 MPa
10900 - 66000 psi
Average value: 275 MPa Grade Count:245
130 - 388.175 MPa

@Temperature -40.0 - 121 °C
18900 - 56300.1 psi

@Temperature -40.0 - 250 °F
Average value: 225 MPa Grade Count:8
Flexural Modulus 1.10 - 113 GPa
160 - 16300 ksi
Average value: 10.5 GPa Grade Count:272
5.00 - 14.0 GPa

@Temperature -40.0 - 121 °C
725 - 2030 ksi

@Temperature -40.0 - 250 °F
Average value: 8.45 GPa Grade Count:8
Compressive Yield Strength 145 - 276 MPa
21000 - 40000 psi
Average value: 211 MPa Grade Count:10
Poissons Ratio 0.350 - 0.400
0.350 - 0.400
Average value: 0.393 Grade Count:7
Fatigue Strength >= 45.0 MPa

@Temperature 150 - 200 °C
>= 6530 psi

@Temperature 302 - 392 °F
Average value: 53.8 MPa Grade Count:1
>= 45.0 MPa

@Time 0.000 - 25200 sec
>= 6530 psi

@Time 0.000 - 7.00 hour
Average value: 53.8 MPa Grade Count:1
Shear Modulus 1.36 - 2.17 GPa
198 - 315 ksi
Average value: 1.78 GPa Grade Count:6
>= 0.293 GPa

@Temperature -50.0 - 250 °C
>= 42.5 ksi

@Temperature -58.0 - 482 °F
Average value: 1.13 GPa Grade Count:6
Shear Strength 72.0 - 90.0 MPa
10400 - 13100 psi
Average value: 81.0 MPa Grade Count:8
Izod Impact, Notched 0.700 - 5.07 J/cm
1.31 - 9.50 ft-lb/in
Average value: 1.57 J/cm Grade Count:133
1.05 - 4.64493 J/cm

@Temperature -40.0 - 149 °C
1.97 - 8.70186 ft-lb/in

@Temperature -40.0 - 300 °F
Average value: 2.82 J/cm Grade Count:4
Izod Impact, Unnotched 1.23 - 16.0 J/cm
2.30 - 30.0 ft-lb/in
Average value: 11.1 J/cm Grade Count:51
Izod Impact, Notched (ISO) 2.50 - 47.0 kJ/m²
1.19 - 22.4 ft-lb/in²
Average value: 14.3 kJ/m² Grade Count:111
8.00 - 64.0 kJ/m²

@Temperature -40.0 - -20.0 °C
3.81 - 30.5 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 13.3 kJ/m² Grade Count:45
Izod Impact, Unnotched (ISO) 55.0 - 105 kJ/m²
26.2 - 50.0 ft-lb/in²
Average value: 77.5 kJ/m² Grade Count:16
50.0 - 105 kJ/m²

@Temperature -40.0 - -30.0 °C
23.8 - 50.0 ft-lb/in²

@Temperature -40.0 - -22.0 °F
Average value: 73.8 kJ/m² Grade Count:9
Charpy Impact Unnotched 3.80 J/cm² - NB
18.1 ft-lb/in² - NB
Average value: 8.46 J/cm² Grade Count:171
3.00 - 999.9 J/cm²

@Temperature -40.0 - 30.0 °C
14.3 - 4759 ft-lb/in²

@Temperature -40.0 - 86.0 °F
Average value: 7.50 J/cm² Grade Count:91
Charpy Impact, Notched 0.600 - 3.60 J/cm²
2.86 - 17.1 ft-lb/in²
Average value: 1.53 J/cm² Grade Count:178
0.500 - 20.0 J/cm²

@Temperature -40.0 - 30.0 °C
2.38 - 95.2 ft-lb/in²

@Temperature -40.0 - 86.0 °F
Average value: 1.31 J/cm² Grade Count:96