Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Nylon 12, Extrusion/Tubing Grade

Category Polymer , Thermoplastic , Nylon , Nylon 12 , Nylon 12, Extrusion/Tubing Grade
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Nylon 12, Extrusion/Tubing Grade.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 12, Extrusion/Tubing Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.00 - 1.04 g/cc
0.0361 - 0.0376 lb/in³
Average value: 1.02 g/cc Grade Count:26
Water Absorption 1.00 - 2.30 %
1.00 - 2.30 %
Average value: 1.41 % Grade Count:9
Moisture Absorption at Equilibrium 0.500 - 0.700 %
0.500 - 0.700 %
Average value: 0.550 % Grade Count:14
Water Absorption at Saturation 1.00 - 1.50 %
1.00 - 1.50 %
Average value: 1.20 % Grade Count:6
Melt Flow 1.90 - 170 g/10 min
1.90 - 170 g/10 min
Average value: 26.4 g/10 min Grade Count:23
Mechanical Properties Metric English Comments
Tensile Strength, Yield 20.0 - 76.0 MPa
2900 - 11000 psi
Average value: 39.5 MPa Grade Count:34
Elongation at Break 50.0 - 400 %
50.0 - 400 %
Average value: 86.7 % Grade Count:39
Elongation at Yield 5.00 - 32.0 %
5.00 - 32.0 %
Average value: 16.1 % Grade Count:30
Modulus of Elasticity 0.350 - 2.23 GPa
50.8 - 323 ksi
Average value: 1.05 GPa Grade Count:34
Charpy Impact Unnotched 1000 J/cm² - NB
4760 ft-lb/in² - NB
Grade Count:27
NB - NB

@Temperature -30.0 - -30.0 °C
NB - NB

@Temperature -22.0 - -22.0 °F
Grade Count:12
Charpy Impact, Notched 0.400 J/cm² - NB
1.90 ft-lb/in² - NB
Average value: 1.85 J/cm² Grade Count:25
0.250 - 1.24 J/cm²

@Temperature -30.0 - -30.0 °C
1.19 - 5.90 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 0.640 J/cm² Grade Count:24
Thermal Properties Metric English Comments
CTE, linear 50.0 - 150 µm/m-°C
27.8 - 83.3 µin/in-°F
Average value: 96.4 µm/m-°C Grade Count:20
CTE, linear, Transverse to Flow 100 µm/m-°C
55.6 µin/in-°F
Average value: 100 µm/m-°C Grade Count:6
Melting Point 168 - 178 °C
334 - 352 °F
Average value: 174 °C Grade Count:14
Maximum Service Temperature, Air 75.0 - 150 °C
167 - 302 °F
Average value: 113 °C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 90.0 - 135 °C
194 - 275 °F
Average value: 113 °C Grade Count:14
Deflection Temperature at 1.8 MPa (264 psi) 40.0 - 165 °C
104 - 329 °F
Average value: 56.3 °C Grade Count:20
Vicat Softening Point 115 - 142 °C
239 - 288 °F
Average value: 131 °C Grade Count:15
Flammability, UL94 HB - V-2
HB - V-2
Grade Count:21
Optical Properties Metric English Comments
Transmission, Visible 80.0 %
80.0 %
Average value: 80.0 % Grade Count:4
Electrical Properties Metric English Comments
Electrical Resistivity 2.00e+8 - 1.00e+15 ohm-cm
2.00e+8 - 1.00e+15 ohm-cm
Average value: 9.97e+13 ohm-cm Grade Count:20
Surface Resistance 1.00e+11 - 1.00e+15 ohm
1.00e+11 - 1.00e+15 ohm
Average value: 3.55e+14 ohm Grade Count:20
Dielectric Constant 3.00 - 15.0
3.00 - 15.0
Average value: 5.83 Grade Count:12
Dielectric Strength 24.0 - 50.0 kV/mm
610 - 1270 kV/in
Average value: 34.7 kV/mm Grade Count:21
Dissipation Factor 0.000304 - 0.330
0.000304 - 0.330
Average value: 0.0916 Grade Count:14
Comparative Tracking Index 575 - 600 V
575 - 600 V
Average value: 597 V Grade Count:17
Processing Properties Metric English Comments
Processing Temperature 230 °C
446 °F
Average value: 230 °C Grade Count:5
Die Temperature 230 °C
446 °F
Average value: 230 °C Grade Count:5
Melt Temperature 190 - 240 °C
374 - 464 °F
Average value: 220 °C Grade Count:5
Mold Temperature 40.0 - 60.0 °C
104 - 140 °F
Average value: 50.0 °C Grade Count:5
Injection Velocity 100 mm/sec
3.94 in/sec
Average value: 100 mm/sec Grade Count:5
Die Opening 0.0400 cm
0.0157 in
Average value: 0.0400 cm Grade Count:5
Roll Temperature 50.0 °C
122 °F
Average value: 50.0 °C Grade Count:5
Drying Temperature 80.0 - 110 °C
176 - 230 °F
Average value: 96.7 °C Grade Count:5
Injection Pressure 40.0 - 50.0 MPa
5800 - 7250 psi
Average value: 45.0 MPa Grade Count:5
Users viewing this material also viewed the following: