Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Solvay Specialty Polymers Amodel® AS-1566 HS Polyphthalamide (PPA), 65% GlassMineral (Dry)

Category Polymer , Thermoplastic , Polyphthalamide (PPA)
Manufacturer Solvay Specialty Polymers
Trade Name Amodel®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Solvay Specialty Polymers Amodel® AS-1566 HS Polyphthalamide (PPA), 65% GlassMineral (Dry).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Amodel® AS-1566 HS resin is a 65% glass and mineral reinforced polyphthalamide (PPA) resin that exhibits a high deflection temperature and high flexural modulus. This grade was designed specifically to be cost effective for most applications requiring high stiffness, good dimensional stability and chemical resistance.Features: Good Chemical Resistance; Good Creep Resistance; Good Dimensional Stability; Good Toughness; Heat Stabilized; High Heat Resistance; High Strength; Low CLTE; Ultra High StiffnessUses: Automotive Applications; Automotive Electronics; Automotive Under the Hood; General Purpose; Housings; Industrial Applications; Industrial Parts; Lawn and Garden Equipment; Machine/Mechanical Parts; Metal Replacement; Power/Other Tools; Thick-walled Parts; Valves/Valve PartsInjection Molding Notes: Amodel® compounds are shipped in moisture-resistant packages at moisture levels according to specifications. Sealed, undamaged bags should be preferably stored in a dry room at a maximum temperature of 50°C (122°F) and should be protected from possible damage. If only a portion of a package is used, the remaining material should be transferred into a sealable container. It is recommended that Amodel® resins be dried prior to molding.Automotive Specifications ASTM D6779 PA122R65 Color: BK324 Black; ASTM D6779 PA122R65 Color: BK545 Black; ASTM D6779 PA122R65 Color: NT Natural; BMW GS 93016; DELPHI DCM4899 Color: BK324 Black; DELPHI DCM4899 Color: NT Natural; DELPHI M-2987 Color: BK324 Black; DELPHI M-2987 Color: NT Natural; DELPHI M-53292; DELPHI M-53292 Color: BK545 Black; GM GM7001M PA6T/6I/66 A3 A22 A42 A64 BJ721 DE1830 KS1750 Color: NT Natural; GM GMP.PPA.003 Color: Black; GM GMP.PPA.003 Color: Natural; GM GMW16358P-PPA-GF43MD22 Color: BK324 Black; GM GMW16358P-PPA-GF43MD22 Color: NT Natural; ISO 1874 PA6T/6I/66, MH, 11-120, (GF+MD)64 Color: BK324 Black; ISO 1874 PA6T/6I/66, MH, 11-120, (GF+MD)64 Color: NT Natural; TRW SP-13161601 Color: BK324 Black; TRW SP-13161601 Color: NT NaturalInformation provided by Solvay Specialty Polymers.
Physical Properties Metric English Comments
Density 1.84 g/cc
0.0665 lb/in³
ISO 1183
Filler Content 65 %
65 %
GlassMineral
Water Absorption 0.10 %

@Time 86400 sec
0.10 %

@Time 24.0 hour
ISO 62
Linear Mold Shrinkage, Flow 0.0030 cm/cm
0.0030 in/in
Linear Mold Shrinkage, Transverse 0.0050 cm/cm
0.0050 in/in
ASTM D955
Mechanical Properties Metric English Comments
Tensile Strength at Break 207 MPa
30000 psi
ASTM D638
43.4 MPa

@Temperature 175 °C
6290 psi

@Temperature 347 °F
ISO 527-2
52.4 MPa

@Temperature 150 °C
7600 psi

@Temperature 302 °F
ISO 527-2
127 MPa

@Temperature 100 °C
18400 psi

@Temperature 212 °F
ISO 527-2
200 MPa

@Temperature 23.0 °C
29000 psi

@Temperature 73.4 °F
ISO 527-2
Elongation at Break 1.7 %
1.7 %
ASTM D638
1.4 %

@Temperature 23.0 °C
1.4 %

@Temperature 73.4 °F
ISO 527-2
1.5 %

@Temperature 100 °C
1.5 %

@Temperature 212 °F
ISO 527-2
3.1 %

@Temperature 175 °C
3.1 %

@Temperature 347 °F
ISO 527-2
3.4 %

@Temperature 150 °C
3.4 %

@Temperature 302 °F
ISO 527-2
Tensile Modulus 20.0 GPa
2900 ksi
ASTM D638
6.21 GPa

@Temperature 175 °C
901 ksi

@Temperature 347 °F
4; ISO 527-2
7.31 GPa

@Temperature 150 °C
1060 ksi

@Temperature 302 °F
4; ISO 527-2
17.2 GPa

@Temperature 100 °C
2490 ksi

@Temperature 212 °F
4; ISO 527-2
22.5 GPa

@Temperature 23.0 °C
3260 ksi

@Temperature 73.4 °F
4; ISO 527-2
Flexural Strength 75.8 MPa

@Temperature 175 °C
11000 psi

@Temperature 347 °F
4; ISO 178
95.8 MPa

@Temperature 150 °C
13900 psi

@Temperature 302 °F
4; ISO 178
205 MPa

@Temperature 100 °C
29700 psi

@Temperature 212 °F
4; ISO 178
284 MPa

@Temperature 23.0 °C
41200 psi

@Temperature 73.4 °F
4; ISO 178
Flexural Yield Strength 290 MPa
42100 psi
ASTM D790
Flexural Modulus 18.6 GPa
2700 ksi
ASTM D790
6.41 GPa

@Temperature 175 °C
930 ksi

@Temperature 347 °F
ISO 178
7.31 GPa

@Temperature 150 °C
1060 ksi

@Temperature 302 °F
ISO 178
16.8 GPa

@Temperature 100 °C
2440 ksi

@Temperature 212 °F
ISO 178
20.5 GPa

@Temperature 23.0 °C
2970 ksi

@Temperature 73.4 °F
ISO 178
Shear Strength 80.0 MPa
11600 psi
ASTM D732
Izod Impact, Notched 0.640 J/cm
1.20 ft-lb/in
ASTM D256
Izod Impact, Unnotched 5.90 J/cm
11.1 ft-lb/in
ASTM D256
Izod Impact, Notched (ISO) 6.50 kJ/m²
3.09 ft-lb/in²
Type 1, Notch A; ISO 180
Izod Impact, Unnotched (ISO) 44.0 kJ/m²
20.9 ft-lb/in²
Type 1; ISO 180
Charpy Impact Unnotched 3.40 J/cm²
16.2 ft-lb/in²
Type 1, Edgewise; ISO 179
Charpy Impact, Notched 0.610 J/cm²
2.90 ft-lb/in²
Type 1, Edgewise; ISO 179
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 17.0 µm/m-°C

@Temperature 100 - 200 °C
9.44 µin/in-°F

@Temperature 212 - 392 °F
2
17.0 µm/m-°C

@Temperature 0.000 - 100 °C
9.44 µin/in-°F

@Temperature 32.0 - 212 °F
2
CTE, linear, Transverse to Flow 40.0 µm/m-°C

@Temperature 0.000 - 100 °C
22.2 µin/in-°F

@Temperature 32.0 - 212 °F
TMA; ASTM E831
72.0 µm/m-°C

@Temperature 100 - 200 °C
40.0 µin/in-°F

@Temperature 212 - 392 °F
TMA; ASTM E831
Melting Point 311 °C
592 °F
ASTM D3418
311 °C
592 °F
ISO 11357-3
Deflection Temperature at 1.8 MPa (264 psi) 278 °C
532 °F
Annealed; ASTM D648
280 °C
536 °F
Unannealed; ISO 75-2/A
Processing Properties Metric English Comments
Processing Temperature 79.4 °C
175 °F
Hopper
Rear Barrel Temperature 307 - 329 °C
585 - 624 °F
Front Barrel Temperature 307 - 329 °C
585 - 624 °F
Melt Temperature 321 - 343 °C
610 - 649 °F
Mold Temperature 65.6 - 166 °C
150 - 331 °F
Drying Temperature 120 °C

@Time 14400 sec
248 °F

@Time 4.00 hour
Moisture Content <= 0.045 %
<= 0.045 %
Descriptive Properties Value Comments
Additive Heat Stabilizer
Availability Africa & Middle East
Asia Pacific
Europe
Latin America
North America
Color Black; Natural
Form Pellets
Processing Technique Injection Molding
RoHS Compliance RoHS Compliant
Users viewing this material also viewed the following: