| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.29 g/cc | 0.0466 lb/in³ | ISO 1183 |
| 1.30 g/cc | 0.0470 lb/in³ | ASTM D792 | |
| Linear Mold Shrinkage, Flow | 0.0028 cm/cm @Time 86400 sec |
0.0028 in/in @Time 24.0 hour |
ISO 294 |
| 0.0020 - 0.0040 cm/cm @Time 86400 sec |
0.0020 - 0.0040 in/in @Time 24.0 hour |
ASTM D955 | |
| Linear Mold Shrinkage, Transverse | 0.0049 cm/cm @Time 86400 sec |
0.0049 in/in @Time 24.0 hour |
ISO 294 |
| 0.0040 - 0.0060 cm/cm @Time 86400 sec |
0.0040 - 0.0060 in/in @Time 24.0 hour |
ASTM D955 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 84.0 MPa | 12200 psi | ISO 527 |
| 88.0 MPa | 12800 psi | ASTM D638 | |
| Tensile Strength, Yield | 84.0 MPa | 12200 psi | ISO 527 |
| 88.0 MPa | 12800 psi | ASTM D638 | |
| Elongation at Break | 1.6 % | 1.6 % | ISO 527 |
| 1.7 % | 1.7 % | ASTM D638 | |
| Elongation at Yield | 1.6 % | 1.6 % | ISO 527 |
| 1.7 % | 1.7 % | ASTM D638 | |
| Tensile Modulus | 6.83 GPa | 991 ksi | 1 mm/min; ISO 527 |
| 6.89 GPa | 999 ksi | 50 mm/min; ASTM D638 | |
| Flexural Strength | 118 MPa | 17100 psi | ISO 178 |
| 241 MPa | 35000 psi | ASTM D790 | |
| Flexural Modulus | 6.60 GPa | 957 ksi | ISO 178 |
| 12.41 GPa | 1800 ksi | ASTM D790 | |
| Izod Impact, Notched | 0.800 J/cm | 1.50 ft-lb/in | ASTM D256 |
| Izod Impact, Unnotched | 4.16 J/cm | 7.79 ft-lb/in | ASTM D4812 |
| Izod Impact, Notched (ISO) | 7.00 kJ/m² | 3.33 ft-lb/in² | 80*10*4; ISO 180/1A |
| Izod Impact, Unnotched (ISO) | 25.0 kJ/m² | 11.9 ft-lb/in² | 80*10*4; ISO 180/1U |
| Dart Drop, Total Energy | 14.0 J | 10.3 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
| Impact Test | 3.00 J | 2.21 ft-lb | Multiaxial Impact; ISO 6603 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 57.6 µm/m-°C @Temperature -40.0 - 40.0 °C |
32.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 58.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
32.2 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| CTE, linear, Transverse to Flow | 39.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
21.7 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 |
| 39.6 µm/m-°C @Temperature -40.0 - 40.0 °C |
22.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 | |
| Deflection Temperature at 0.46 MPa (66 psi) | 111 °C | 232 °F | Flatw 80*10*4 sp=64mm; ISO 75/Bf |
| 110 °C @Thickness 3.20 mm |
230 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
| Deflection Temperature at 1.8 MPa (264 psi) | 104 °C | 219 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
| 102 °C @Thickness 3.20 mm |
216 °F @Thickness 0.126 in |
unannealed; ASTM D648 |