Material Notes:
Age-hardenable, high ductility in the aged condition, lower thermal expansion than most alloys, very good oxidation resistance up to 815°C, excellent low cycle fatigue properties, very good thermal stability, and resistance to high-temperature fluorine and fluoride environments. Applications include seal rings, containment rings, duct segments, casings, fasteners, rocket nozzles, pumps, hydrofluoric acid vapor containing processes, fluoroelastomer process equipment such as extrusion screws.Data provided by the manufacturer, Haynes International, Inc.
Physical Properties Metric English Comments
Density 9.05 g/cc
0.327 lb/in³
at RT
Mechanical Properties Metric English Comments
Hardness, Brinell 257
257
Converted from Vickers hardness
Hardness, Knoop 286
286
Converted from Vickers hardness
Hardness, Rockwell C 19
19
Converted from Vickers hardness
Hardness, Vickers 78.0

@Temperature 870 °C
78.0

@Temperature 1600 °F
140

@Temperature 760 °C
140

@Temperature 1400 °F
218

@Temperature 650 °C
218

@Temperature 1200 °F
263

@Temperature 540 °C
263

@Temperature 1000 °F
271

@Temperature 425 °C
271

@Temperature 797 °F
Tensile Strength, Ultimate 1290 MPa
187000 psi
290 MPa

@Temperature 980 °C
42100 psi

@Temperature 1800 °F
500 MPa

@Temperature 870 °C
72500 psi

@Temperature 1600 °F
730 MPa

@Temperature 760 °C
106000 psi

@Temperature 1400 °F
1000 MPa

@Temperature 650 °C
145000 psi

@Temperature 1200 °F
1080 MPa

@Temperature 540 °C
157000 psi

@Temperature 1000 °F
1110 MPa

@Temperature 425 °C
161000 psi

@Temperature 797 °F
1160 MPa

@Temperature 315 °C
168000 psi

@Temperature 599 °F
1195 MPa

@Temperature 205 °C
173300 psi

@Temperature 401 °F
1245 MPa

@Temperature 95.0 °C
180600 psi

@Temperature 203 °F
Tensile Strength, Yield 845 MPa

@Strain 0.200 %
123000 psi

@Strain 0.200 %
210 MPa

@Strain 0.200 %,
Temperature 980 °C
30500 psi

@Strain 0.200 %,
Temperature 1800 °F
310 MPa

@Strain 0.200 %,
Temperature 760 °C
45000 psi

@Strain 0.200 %,
Temperature 1400 °F
310 MPa

@Strain 0.200 %,
Temperature 870 °C
45000 psi

@Strain 0.200 %,
Temperature 1600 °F
540 MPa

@Strain 0.200 %,
Temperature 540 °C
78300 psi

@Strain 0.200 %,
Temperature 1000 °F
570 MPa

@Strain 0.200 %,
Temperature 650 °C
82700 psi

@Strain 0.200 %,
Temperature 1200 °F
595 MPa

@Strain 0.200 %,
Temperature 425 °C
86300 psi

@Strain 0.200 %,
Temperature 797 °F
665 MPa

@Strain 0.200 %,
Temperature 315 °C
96500 psi

@Strain 0.200 %,
Temperature 599 °F
705 MPa

@Strain 0.200 %,
Temperature 205 °C
102000 psi

@Strain 0.200 %,
Temperature 401 °F
760 MPa

@Strain 0.200 %,
Temperature 95.0 °C
110000 psi

@Strain 0.200 %,
Temperature 203 °F
Elongation at Break 33.7 %
33.7 %
in 4D
31.7 %

@Temperature 95.0 °C
31.7 %

@Temperature 203 °F
in 4D
33 %

@Temperature 205 °C
33 %

@Temperature 401 °F
in 4D
33.2 %

@Temperature 650 °C
33.2 %

@Temperature 1200 °F
in 4D
33.4 %

@Temperature 315 °C
33.4 %

@Temperature 599 °F
in 4D
37.6 %

@Temperature 425 °C
37.6 %

@Temperature 797 °F
in 4D
38.3 %

@Temperature 540 °C
38.3 %

@Temperature 1000 °F
in 4D
44.3 %

@Temperature 760 °C
44.3 %

@Temperature 1400 °F
in 4D
49.7 %

@Temperature 870 °C
49.7 %

@Temperature 1600 °F
in 4D
54 %

@Temperature 980 °C
54 %

@Temperature 1800 °F
in 4D
Reduction of Area 45.7 %
45.7 %
41.1 %

@Temperature 650 °C
41.1 %

@Temperature 1200 °F
45.9 %

@Temperature 425 °C
45.9 %

@Temperature 797 °F
47 %

@Temperature 95.0 °C
47 %

@Temperature 203 °F
48.4 %

@Temperature 315 °C
48.4 %

@Temperature 599 °F
49.9 %

@Temperature 540 °C
49.9 %

@Temperature 1000 °F
51.8 %

@Temperature 205 °C
51.8 %

@Temperature 401 °F
54.1 %

@Temperature 760 °C
54.1 %

@Temperature 1400 °F
85.1 %

@Temperature 870 °C
85.1 %

@Temperature 1600 °F
97.8 %

@Temperature 980 °C
97.8 %

@Temperature 1800 °F
Modulus of Elasticity 229 GPa
33200 ksi
RT
152 GPa

@Temperature 1000 °C
22000 ksi

@Temperature 1830 °F
163 GPa

@Temperature 900 °C
23600 ksi

@Temperature 1650 °F
172 GPa

@Temperature 800 °C
24900 ksi

@Temperature 1470 °F
185 GPa

@Temperature 700 °C
26800 ksi

@Temperature 1290 °F
193 GPa

@Temperature 600 °C
28000 ksi

@Temperature 1110 °F
199 GPa

@Temperature 500 °C
28900 ksi

@Temperature 932 °F
206 GPa

@Temperature 400 °C
29900 ksi

@Temperature 752 °F
213 GPa

@Temperature 300 °C
30900 ksi

@Temperature 572 °F
219 GPa

@Temperature 200 °C
31800 ksi

@Temperature 392 °F
225 GPa

@Temperature 100 °C
32600 ksi

@Temperature 212 °F
Thermal Properties Metric English Comments
CTE, linear 10.8 µm/m-°C

@Temperature 25.0 - 100 °C
6.00 µin/in-°F

@Temperature 77.0 - 212 °F
11.3 µm/m-°C

@Temperature 25.0 - 200 °C
6.28 µin/in-°F

@Temperature 77.0 - 392 °F
11.6 µm/m-°C

@Temperature 25.0 - 300 °C
6.44 µin/in-°F

@Temperature 77.0 - 572 °F
11.9 µm/m-°C

@Temperature 25.0 - 400 °C
6.61 µin/in-°F

@Temperature 77.0 - 752 °F
12.2 µm/m-°C

@Temperature 25.0 - 500 °C
6.78 µin/in-°F

@Temperature 77.0 - 932 °F
Electrical Properties Metric English Comments
Electrical Resistivity 0.000122 ohm-cm
0.000122 ohm-cm
RT
0.0001234 ohm-cm

@Temperature 100 °C
0.0001234 ohm-cm

@Temperature 212 °F
0.0001251 ohm-cm

@Temperature 200 °C
0.0001251 ohm-cm

@Temperature 392 °F
0.0001267 ohm-cm

@Temperature 300 °C
0.0001267 ohm-cm

@Temperature 572 °F
0.0001276 ohm-cm

@Temperature 1000 °C
0.0001276 ohm-cm

@Temperature 1830 °F
0.000128 ohm-cm

@Temperature 400 °C
0.000128 ohm-cm

@Temperature 752 °F
0.0001295 ohm-cm

@Temperature 500 °C
0.0001295 ohm-cm

@Temperature 932 °F
0.0001298 ohm-cm

@Temperature 900 °C
0.0001298 ohm-cm

@Temperature 1650 °F
0.0001306 ohm-cm

@Temperature 600 °C
0.0001306 ohm-cm

@Temperature 1110 °F
0.000132 ohm-cm

@Temperature 700 °C
0.000132 ohm-cm

@Temperature 1290 °F
0.0001324 ohm-cm

@Temperature 800 °C
0.0001324 ohm-cm

@Temperature 1470 °F