Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Nylon 6, Glass Filled, Impact Grade

Category Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, Glass Filled, Impact Grade
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Nylon 6, Glass Filled, Impact Grade.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Glass Filled, Impact Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.15 - 1.53 g/cc
0.0415 - 0.0553 lb/in³
Average value: 1.29 g/cc Grade Count:98
Filler Content 5.00 - 50.0 %
5.00 - 50.0 %
Average value: 27.0 % Grade Count:10
Water Absorption 0.600 - 7.00 %
0.600 - 7.00 %
Average value: 1.98 % Grade Count:45
Moisture Absorption at Equilibrium 1.40 - 2.50 %
1.40 - 2.50 %
Average value: 1.89 % Grade Count:34
Water Absorption at Saturation 4.80 - 8.50 %
4.80 - 8.50 %
Average value: 6.22 % Grade Count:18
Viscosity Test 150 cm³/g
150 cm³/g
Average value: 150 cm³/g Grade Count:3
Linear Mold Shrinkage 0.000600 - 0.0135 cm/cm
0.000600 - 0.0135 in/in
Average value: 0.00401 cm/cm Grade Count:82
Linear Mold Shrinkage, Transverse 0.00100 - 0.0140 cm/cm
0.00100 - 0.0140 in/in
Average value: 0.00752 cm/cm Grade Count:33
Melt Flow 1.00 - 45.0 g/10 min
1.00 - 45.0 g/10 min
Average value: 25.3 g/10 min Grade Count:4
Ash 30.0 - 30.0 %

@Temperature 650 - 650 °C
30.0 - 30.0 %

@Temperature 1200 - 1200 °F
Average value: 30.0 % Grade Count:1
Mechanical Properties Metric English Comments
Hardness, Rockwell M 76.0 - 121
76.0 - 121
Average value: 83.9 Grade Count:13
Hardness, Rockwell R 110 - 120
110 - 120
Average value: 117 Grade Count:23
Ball Indentation Hardness 55.0 - 195 MPa
7980 - 28300 psi
Average value: 126 MPa Grade Count:4
Tensile Strength, Ultimate 40.0 - 190 MPa
5800 - 27600 psi
Average value: 113 MPa Grade Count:90
Tensile Strength, Yield 6.00 - 170 MPa
870 - 24700 psi
Average value: 105 MPa Grade Count:16
Elongation at Break 2.20 - 28.0 %
2.20 - 28.0 %
Average value: 5.41 % Grade Count:93
Elongation at Yield 2.00 - 5.50 %
2.00 - 5.50 %
Average value: 3.94 % Grade Count:10
Modulus of Elasticity 0.930 - 13.8 GPa
135 - 2000 ksi
Average value: 6.49 GPa Grade Count:74
Flexural Yield Strength 55.0 - 290 MPa
7980 - 42100 psi
Average value: 170 MPa Grade Count:75
Flexural Modulus 2.10 - 11.7 GPa
305 - 1700 ksi
Average value: 6.03 GPa Grade Count:78
Compressive Yield Strength 62.1 - 172 MPa
9000 - 24900 psi
Average value: 119 MPa Grade Count:14
Poissons Ratio 0.350
0.350
Average value: 0.350 Grade Count:11
Shear Modulus 1.60 - 4.40 GPa
232 - 638 ksi
Average value: 3.15 GPa Grade Count:8
Izod Impact, Notched 0.640 - 2.14 J/cm
1.20 - 4.00 ft-lb/in
Average value: 1.54 J/cm Grade Count:30
Izod Impact, Unnotched 5.82 J/cm - NB
10.9 ft-lb/in - NB
Average value: 10.1 J/cm Grade Count:13
Izod Impact, Notched (ISO) 10.0 - 50.0 kJ/m²
4.76 - 23.8 ft-lb/in²
Average value: 19.1 kJ/m² Grade Count:23
7.00 - 18.0 kJ/m²

@Temperature -40.0 - -20.0 °C
3.33 - 8.57 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 11.0 kJ/m² Grade Count:18
Izod Impact, Unnotched (ISO) 45.0 - 95.0 kJ/m²
21.4 - 45.2 ft-lb/in²
Average value: 72.0 kJ/m² Grade Count:18
35.0 - 90.0 kJ/m²

@Temperature -30.0 - -30.0 °C
16.7 - 42.8 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 64.9 kJ/m² Grade Count:16
Charpy Impact Unnotched 5.00 J/cm² - NB
23.8 ft-lb/in² - NB
Average value: 8.67 J/cm² Grade Count:41
4.50 - 11.5 J/cm²

@Temperature -40.0 - -20.0 °C
21.4 - 54.7 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 7.57 J/cm² Grade Count:27
Charpy Impact, Notched 0.700 - 4.20 J/cm²
3.33 - 20.0 ft-lb/in²
Average value: 2.13 J/cm² Grade Count:47
0.610 - 2.00 J/cm²

@Temperature -30.0 - -20.0 °C
2.90 - 9.52 ft-lb/in²

@Temperature -22.0 - -4.00 °F
Average value: 1.17 J/cm² Grade Count:30
Puncture Energy 3.80 - 32.0 J
2.80 - 23.6 ft-lb
Average value: 11.4 J Grade Count:4
2.50 - 4.80 J

@Temperature -30.0 - -30.0 °C
1.84 - 3.54 ft-lb

@Temperature -22.0 - -22.0 °F
Average value: 3.10 J Grade Count:4
2.50 - 4.80 J

@Load <=78.5 kg
1.84 - 3.54 ft-lb

@Load <=173 lb
Average value: 3.10 J Grade Count:4
Thermal Properties Metric English Comments
CTE, linear 19.0 - 52.0 µm/m-°C
10.6 - 28.9 µin/in-°F
Average value: 30.5 µm/m-°C Grade Count:29
CTE, linear, Transverse to Flow 65.0 - 180 µm/m-°C
36.1 - 100 µin/in-°F
Average value: 104 µm/m-°C Grade Count:17
Thermal Conductivity 0.200 - 0.389 W/m-K
1.39 - 2.70 BTU-in/hr-ft²-°F
Average value: 0.312 W/m-K Grade Count:3
Melting Point 205 - 225 °C
401 - 437 °F
Average value: 218 °C Grade Count:73
Deflection Temperature at 0.46 MPa (66 psi) 180 - 220 °C
356 - 428 °F
Average value: 210 °C Grade Count:63
Deflection Temperature at 1.8 MPa (264 psi) 70.0 - 213 °C
158 - 415 °F
Average value: 193 °C Grade Count:78
Vicat Softening Point 170 - 215 °C
338 - 419 °F
Average value: 198 °C Grade Count:23
Flammability, UL94 HB
HB
Grade Count:53
Glow Wire Test 550 - 650 °C
1020 - 1200 °F
Average value: 607 °C Grade Count:7
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+12 - 1.00e+15 ohm-cm
1.00e+12 - 1.00e+15 ohm-cm
Average value: 4.45e+14 ohm-cm Grade Count:35
Surface Resistance 1.00e+10 - 1.00e+16 ohm
1.00e+10 - 1.00e+16 ohm
Average value: 1.56e+15 ohm Grade Count:19
Dielectric Constant 3.20 - 14.0
3.20 - 14.0
Average value: 5.65 Grade Count:21
Dielectric Strength 19.7 - 43.0 kV/mm
500 - 1090 kV/in
Average value: 31.2 kV/mm Grade Count:24
Dissipation Factor 0.00600 - 0.300
0.00600 - 0.300
Average value: 0.0817 Grade Count:9
Dielectric Loss Index 0.0200 - 0.220
0.0200 - 0.220
Average value: 0.113 Grade Count:12
Arc Resistance 120 - 180 sec
120 - 180 sec
Average value: 150 sec Grade Count:4
Comparative Tracking Index 450 - 600 V
450 - 600 V
Average value: 557 V Grade Count:17
Processing Properties Metric English Comments
Processing Temperature 221 - 290 °C
430 - 554 °F
Average value: 263 °C Grade Count:22
Melt Temperature 220 - 291 °C
428 - 556 °F
Average value: 260 °C Grade Count:47
Mold Temperature 50.0 - 121 °C
122 - 250 °F
Average value: 81.6 °C Grade Count:64