Material Notes:
LNP* THERMOCOMP* EC008PXQ is a compound based on Polyetherimide containing 40% Carbon FIber. Added features include: Electrically Conductive, Exceptional Processing
Physical Properties Metric English Comments
Specific Gravity 1.44 g/cc
1.44 g/cc
ASTM D792
Density 1.43 g/cc
0.0517 lb/in³
ASTM D792
Moisture Absorption 0.110 %
0.110 %
50% RH, 24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.00010 - 0.00050 cm/cm

@Time 86400 sec
0.00010 - 0.00050 in/in

@Time 24.0 hour
ASTM D955
Linear Mold Shrinkage, Transverse 0.0010 - 0.0050 cm/cm

@Time 86400 sec
0.0010 - 0.0050 in/in

@Time 24.0 hour
ASTM D955
Melt Flow 15 g/10 min

@Load 6.70 kg,
Temperature 380 °C
15 g/10 min

@Load 14.8 lb,
Temperature 716 °F
ASTM D1238
Mechanical Properties Metric English Comments
Hardness, Rockwell M 112
112
ASTM D785
Tensile Strength at Break 247 MPa
35800 psi
5 mm/min; ISO 527
272 MPa
39500 psi
Type I, 5 mm/min; ASTM D638
Elongation at Break 0.90 %
0.90 %
5 mm/min; ISO 527
1.0 %
1.0 %
Type I, 5 mm/min; ASTM D638
Tensile Modulus 35.48 GPa
5146 ksi
1 mm/min; ISO 527
38.6 GPa
5600 ksi
5 mm/min; ASTM D638
Flexural Strength 364 MPa
52800 psi
2 mm/min; ISO 178
372 MPa
54000 psi
1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 30.56 GPa
4432 ksi
2 mm/min; ISO 178
32.6 GPa
4730 ksi
1.3 mm/min, 50 mm span; ASTM D790
Compressive Strength 222 MPa
32200 psi
SABIC Method
Poissons Ratio 0.40
0.40
ASTM E 132
Shear Modulus 4.656 GPa
675.3 ksi
ASTM C273
Shear Strength 120 MPa
17400 psi
ASTM C273
Izod Impact, Notched 0.740 J/cm
1.39 ft-lb/in
ASTM D256
Izod Impact, Unnotched 5.97 J/cm
11.2 ft-lb/in
ASTM D4812
Izod Impact, Notched (ISO) 6.00 kJ/m²
2.86 ft-lb/in²
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 33.0 kJ/m²
15.7 ft-lb/in²
80*10*4; ISO 180/1U
Dart Drop, Total Energy 7.00 J

@Temperature 23.0 °C
5.16 ft-lb

@Temperature 73.4 °F
ASTM D3763
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 2.70 µm/m-°C

@Temperature -40.0 - 150 °C
1.50 µin/in-°F

@Temperature -40.0 - 302 °F
ASTM E 831
CTE, linear, Transverse to Flow 36.0 µm/m-°C

@Temperature -40.0 - 150 °C
20.0 µin/in-°F

@Temperature -40.0 - 302 °F
ASTM E 831
Deflection Temperature at 1.8 MPa (264 psi) 193 °C

@Thickness 3.20 mm
379 °F

@Thickness 0.126 in
unannealed; ASTM D648
Electrical Properties Metric English Comments
Volume Resistivity 450 ohm-cm
450 ohm-cm
ASTM D257
Surface Resistance 4100 ohm
4100 ohm
ASTM D257