Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Nylon 66, Heat Stabilized

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, Heat Stabilized
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Overview of materials for Nylon 66, Heat Stabilized.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, Heat Stabilized". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.04 - 1.85 g/cc
0.0376 - 0.0668 lb/in³
Average value: 1.31 g/cc Grade Count:378
Filler Content 15.0 - 60.0 %
15.0 - 60.0 %
Average value: 33.7 % Grade Count:34
Water Absorption 0.300 - 8.50 %
0.300 - 8.50 %
Average value: 1.15 % Grade Count:231
Moisture Absorption at Equilibrium 0.250 - 2.80 %
0.250 - 2.80 %
Average value: 1.86 % Grade Count:35
Water Absorption at Saturation 2.50 - 10.0 %
2.50 - 10.0 %
Average value: 5.90 % Grade Count:44
Linear Mold Shrinkage 0.00100 - 0.0335 cm/cm
0.00100 - 0.0335 in/in
Average value: 0.00803 cm/cm Grade Count:359
Linear Mold Shrinkage, Transverse 0.00130 - 0.0240 cm/cm
0.00130 - 0.0240 in/in
Average value: 0.0117 cm/cm Grade Count:88
Melt Flow 1.00 - 50.0 g/10 min
1.00 - 50.0 g/10 min
Average value: 6.53 g/10 min Grade Count:20
Spiral Flow 0.800 - 117 cm
0.315 - 46.1 in
Average value: 83.0 cm Grade Count:21
Mechanical Properties Metric English Comments
Hardness, Rockwell L 110 - 115
110 - 115
Average value: 113 Grade Count:8
Hardness, Rockwell M 55.0 - 119
55.0 - 119
Average value: 78.9 Grade Count:29
Hardness, Rockwell R 82.0 - 122
82.0 - 122
Average value: 114 Grade Count:189
Ball Indentation Hardness 200 - 330 MPa
29000 - 47900 psi
Average value: 255 MPa Grade Count:12
Tensile Strength, Ultimate 34.5 - 300 MPa
5000 - 43500 psi
Average value: 118 MPa Grade Count:164
40.0 - 140 MPa
<br>@Temperature 60.0 - 150 °C
5800 - 20300 psi
<br>@Temperature 140 - 302 °F
Average value: 78.1 MPa Grade Count:5
Tensile Strength, Yield 10.3 - 252 MPa
1500 - 36500 psi
Average value: 119 MPa Grade Count:235
144.79 - 144.79 MPa
<br>@Temperature 93.3 - 93.3 °C
21000 - 21000 psi
<br>@Temperature 200 - 200 °F
Average value: 145 MPa Grade Count:1
Elongation at Break 1.00 - 300 %
1.00 - 300 %
Average value: 21.9 % Grade Count:331
3.20 - 80.0 %
<br>@Temperature 60.0 - 150 °C
3.20 - 80.0 %
<br>@Temperature 140 - 302 °F
Average value: 72.6 % Grade Count:5
Elongation at Yield 2.50 - 90.0 %
2.50 - 90.0 %
Average value: 17.4 % Grade Count:40
Modulus of Elasticity 1.10 - 28.0 GPa
160 - 4060 ksi
Average value: 7.84 GPa Grade Count:105
0.400 - 9.20 GPa
<br>@Temperature 60.0 - 150 °C
58.0 - 1330 ksi
<br>@Temperature 140 - 302 °F
Average value: 2.28 GPa Grade Count:5
Flexural Yield Strength 20.0 - 420 MPa
2900 - 60900 psi
Average value: 174 MPa Grade Count:331
35.0 - 35.0 MPa
<br>@Temperature 90.0 - 90.0 °C
5080 - 5080 psi
<br>@Temperature 194 - 194 °F
Average value: 35.0 MPa Grade Count:1
Flexural Modulus 0.255 - 36.2 GPa
37.0 - 5250 ksi
Average value: 6.54 GPa Grade Count:334
0.750 - 15.1685 GPa
<br>@Temperature 90.0 - 93.3 °C
109 - 2200.03 ksi
<br>@Temperature 194 - 200 °F
Average value: 7.96 GPa Grade Count:2
Compressive Yield Strength 30.3 - 110 MPa
4400 - 16000 psi
Average value: 57.0 MPa Grade Count:3
Poissons Ratio 0.350 - 0.400
0.350 - 0.400
Average value: 0.363 Grade Count:4
Shear Strength 50.0 - 76.5 MPa
7250 - 11100 psi
Average value: 61.7 MPa Grade Count:5
Izod Impact, Notched 0.320 - 10.1 J/cm
0.600 - 19.0 ft-lb/in
Average value: 1.57 J/cm Grade Count:274
0.5339 - 2.6695 J/cm
<br>@Temperature -40.0 - -40.0 °C
1.000 - 5.0011 ft-lb/in
<br>@Temperature -40.0 - -40.0 °F
Average value: 1.29 J/cm Grade Count:16
0.5339 - 2.6695 J/cm
<br>@Thickness 3.17 - 3.17 mm
1.000 - 5.0011 ft-lb/in
<br>@Thickness 0.125 - 0.125 in
Average value: 1.29 J/cm Grade Count:16
Izod Impact, Unnotched 3.20 - 5340 J/cm
6.00 - 10000 ft-lb/in
Average value: 9.26 J/cm Grade Count:75
Izod Impact, Notched (ISO) 3.50 - 861 kJ/m²
1.67 - 410 ft-lb/in²
Average value: 33.0 kJ/m² Grade Count:39
3.50 - 17.0 kJ/m²
<br>@Temperature -40.0 - -20.0 °C
1.67 - 8.09 ft-lb/in²
<br>@Temperature -40.0 - -4.00 °F
Average value: 8.86 kJ/m² Grade Count:31
Izod Impact, Unnotched (ISO) 30.0 - 100 kJ/m²
14.3 - 47.6 ft-lb/in²
Average value: 68.2 kJ/m² Grade Count:13
25.0 - 90.0 kJ/m²
<br>@Temperature -30.0 - -30.0 °C
11.9 - 42.8 ft-lb/in²
<br>@Temperature -22.0 - -22.0 °F
Average value: 62.5 kJ/m² Grade Count:12
Charpy Impact Unnotched 1.30 J/cm² - NB
6.19 ft-lb/in² - NB
Average value: 8.32 J/cm² Grade Count:79
3.20 J/cm² - NB
<br>@Temperature -30.0 - -20.0 °C
15.2 ft-lb/in² - NB
<br>@Temperature -22.0 - -4.00 °F
Average value: 6.99 J/cm² Grade Count:49
Charpy Impact, Notched 0.300 - 3.00 J/cm²
1.43 - 14.3 ft-lb/in²
Average value: 1.25 J/cm² Grade Count:71
0.200 - 1.90 J/cm²
<br>@Temperature -40.0 - -20.0 °C
0.952 - 9.04 ft-lb/in²
<br>@Temperature -40.0 - -4.00 °F
Average value: 0.924 J/cm² Grade Count:51
Puncture Energy 2.00 - 2.00 J
<br>@Temperature -30.0 - -30.0 °C
1.48 - 1.48 ft-lb
<br>@Temperature -22.0 - -22.0 °F
Average value: 2.00 J Grade Count:1
Coefficient of Friction 0.100 - 0.280
0.100 - 0.280
Average value: 0.225 Grade Count:11
Coefficient of Friction, Static 0.0900 - 0.220
0.0900 - 0.220
Average value: 0.170 Grade Count:11
K (wear) Factor 16.1 - 38.3 x 10<sup>-8</sup> mm³/N-M
8.00 - 19.0 x 10<sup>-10</sup> in³-min/ft-lb-hr
Average value: 31.3 x 10&lt;sup&gt;-8&lt;/sup&gt; mm³/N-M Grade Count:11
Limiting Pressure Velocity 0.596 - 1.54 MPa-m/sec
17000 - 44000 psi-ft/min
Average value: 0.690 MPa-m/sec Grade Count:8
Taber Abrasion, mg/1000 Cycles 5.00 - 7.00
5.00 - 7.00
Average value: 6.00 Grade Count:4
Thermal Properties Metric English Comments
CTE, linear 0.710 - 146 µm/m-°C
0.394 - 81.0 µin/in-°F
Average value: 44.4 µm/m-°C Grade Count:206
Electrical Properties Metric English Comments
Electrical Resistivity 1.00 - 1.00e+17 ohm-cm
1.00 - 1.00e+17 ohm-cm
Average value: 2.93e+15 ohm-cm Grade Count:243
Surface Resistance 1.00 - 1.00e+16 ohm
1.00 - 1.00e+16 ohm
Average value: 9.40e+14 ohm Grade Count:113
Dielectric Constant 3.20 - 13.0
3.20 - 13.0
Average value: 4.01 Grade Count:30
Dielectric Strength 15.7 - 120 kV/mm
400 - 3050 kV/in
Average value: 23.4 kV/mm Grade Count:200
Dissipation Factor 0.00680 - 0.320
0.00680 - 0.320
Average value: 0.0302 Grade Count:13
Arc Resistance 95.0 - 185 sec
95.0 - 185 sec
Average value: 127 sec Grade Count:6
Comparative Tracking Index 225 - 600 V
225 - 600 V
Average value: 477 V Grade Count:68
Copyright © lookpolymers.com All Rights Reserved