Tra-Con Tra-Bond F109CLR Fiber Optic Epoxy Adhesive

Category Polymer , Adhesive , Thermoset , Epoxy
Manufacturer Tra-Con, Inc.
Trade Name Tra-Bond
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Tra-Con Tra-Bond F109CLR Fiber Optic Epoxy Adhesive.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
TRA-BOND F109CLR is a clear, low viscosity epoxy specially designed for terminating plastic fibers. This blush free epoxy is an excellent choice for high humidity environments where absolute clarity is essential. This two-part system remains at a constant viscosity for a minimum of 50 minutes. This allows more connectors to be produced from a single lot. It is a very high strength adhesive that will not distort plastic fibers. TRA-BOND F109CLR can be cured at room temperature overnight or as fast as 20 minutes at 65°C. This 100% solid system can be used for small potting and sealing applications where thermal shock and impact resistance are required. Fully cured TRA-BOND F109CLR provides excellent resistance to salt solutions, mild acids, alkalis and many other chemicals including petroleum solvents and alcohol. TRA-BOND F109CLR can be supplied in a wide variety of packages including 2 gram (or large) BIPAX kits, pre-mixed and frozen syringes and 1 gram MINPAX. Sufficient cure is developed for polishing connectors in 20 minutes at 65°C. TRA-BOND F109CLR will complete its cure at room temperature with no pistoning.Information provided by Tra-Con Inc.
Physical Properties Metric English Comments
Specific Gravity 1.14 g/cc
1.14 g/cc
Mixed
Viscosity 300 cP

@Temperature 25.0 °C
300 cP

@Temperature 77.0 °F
After mixing
Mechanical Properties Metric English Comments
Hardness, Shore D 80
80
Adhesive Bond Strength 20.7 MPa
3000 psi
Lap shear, alum to alum
Izod Impact, Notched 0.117 J/cm
0.220 ft-lb/in
Thermal Properties Metric English Comments
CTE, linear 60.0 µm/m-°C

@Temperature 20.0 °C
33.3 µin/in-°F

@Temperature 68.0 °F
Maximum Service Temperature, Air 110 °C
230 °F
Minimum Service Temperature, Air -60.0 °C
-76.0 °F
Glass Transition Temp, Tg 60.0 °C
140 °F
Ultimate Tg
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+11 ohm-cm
1.00e+11 ohm-cm
Dielectric Constant 4.8

@Frequency 1000 Hz
4.8

@Frequency 1000 Hz
Dielectric Strength 16.9 kV/mm
430 kV/in
Processing Properties Metric English Comments
Cure Time 15.0 min

@Temperature 90.0 °C
0.250 hour

@Temperature 194 °F
1 drop applications
60.0 min

@Temperature 65.0 °C
1.00 hour

@Temperature 149 °F
1440 min

@Temperature 25.0 °C
24.0 hour

@Temperature 77.0 °F
Pot Life 20 min
20 min
2 grams
25 min
25 min
25 grams
Descriptive Properties Value Comments
Color Clear
Mix Ratio, parts by weight 100/50
Resin/Hardener
Thixotropic Index 1
Working Life hours 1
2 grams
Working Life minutes 30
25 grams