| Category | Polymer , Thermoplastic , Polyester, TP , Polycyclohexylenedimethylene Terephthalate (PCT) , Glycol-Modified PCT (PCTG) Copolyester |
| Manufacturer | Eastman Chemical |
| Trade Name | DuraStar |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Eastman DuraStar MN611 Polymer, Natural.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.20 g/cc | 1.20 g/cc | ASTM D792 |
| Linear Mold Shrinkage | 0.0020 - 0.0060 cm/cm <br>@Thickness 3.20 mm |
0.0020 - 0.0060 in/in <br>@Thickness 0.126 in |
ASTM D955 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell R | 103 | 103 | ASTM D785 |
| Tensile Strength at Break | 46.0 MPa | 6670 psi | ISO 527 |
| 51.0 MPa | 7400 psi | ASTM D638 | |
| Tensile Strength, Yield | 47.0 MPa | 6820 psi | ASTM D638 |
| 47.0 MPa | 6820 psi | ISO 527 | |
| Elongation at Break | 200 % | 200 % | ISO 527 |
| 300 % | 300 % | ASTM D638 | |
| Elongation at Yield | 4.0 % | 4.0 % | ISO 527 |
| 5.0 % | 5.0 % | ASTM D638 | |
| Tensile Modulus | 1.80 GPa | 261 ksi | ISO 527 |
| Flexural Strength | 65.0 MPa | 9430 psi | ISO 178 |
| Flexural Yield Strength | 69.0 MPa | 10000 psi | ASTM D790 |
| Flexural Modulus | 1.85 GPa | 268 ksi | ISO 178 |
| 2.00 GPa | 290 ksi | ASTM D790 | |
| Izod Impact, Notched | 0.400 J/cm <br>@Temperature -40.0 °C |
0.749 ft-lb/in <br>@Temperature -40.0 °F |
ASTM D256 |
| 0.800 J/cm <br>@Temperature 23.0 °C |
1.50 ft-lb/in <br>@Temperature 73.4 °F |
ASTM D256 | |
| Izod Impact, Unnotched | NB | NB | ASTM D4812 |
| NB <br>@Temperature -40.0 °C |
NB <br>@Temperature -40.0 °F |
ASTM D4812 | |
| Izod Impact, Notched (ISO) | 4.80 kJ/m² <br>@Temperature -40.0 °C |
2.28 ft-lb/in² <br>@Temperature -40.0 °F |
ISO 180 |
| 7.80 kJ/m² <br>@Temperature 23.0 °C |
3.71 ft-lb/in² <br>@Temperature 73.4 °F |
ISO 180 | |
| Puncture Energy | 42.0 J | 31.0 ft-lb | Puncture Resistance @Max Load, 23°C; ASTM D3763 |
| 48.0 J <br>@Temperature -40.0 °C |
35.4 ft-lb <br>@Temperature -40.0 °F |
Puncture Resistance at Max Load; ASTM D3763 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Deflection Temperature at 0.46 MPa (66 psi) | 74.0 °C | 165 °F | ASTM D648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 65.0 °C | 149 °F | ASTM D648 |
| Optical Properties | Metric | English | Comments |
|---|---|---|---|
| Haze | 0.30 % | 0.30 % | ASTM D1003 |
| Transmission, Visible | 89 % | 89 % | Regular Transmittance; ASTM D1003 |
| 91 % | 91 % | Total Transmittance; ASTM D1003 |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Melt Temperature | 232 - 277 °C | 450 - 531 °F | |
| Mold Temperature | 16.0 - 38.0 °C | 60.8 - 100 °F | |
| Drying Temperature | 71.0 °C | 160 °F | |
| Dry Time | 3 - 4 hour | 3 - 4 hour |