Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Solvay Specialty Polymers KetaSpire® KT-880 GF30 Polyetheretherketone (PEEK), 30% Glass Fiber

Category Polymer , Thermoplastic , Polyketone , Polyetheretherketone (PEEK) , Polyetheretherketone, PEEK, Glass Fiber Filled
Manufacturer Solvay Specialty Polymers
Trade Name KetaSpire®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Solvay Specialty Polymers KetaSpire® KT-880 GF30 Polyetheretherketone (PEEK), 30% Glass Fiber.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
KetaSpire® KT-880 GF30 is the high-flow, 30% glass-fiber reinforced grade of polyetheretherketone (PEEK). This resin offers higher strength and stiffness properties relative to unreinforced KetaSpire® PEEK resin. Reinforcement also affords greater mechanical robustness in structural applications, particularly those with service temperatures approaching 300°C.Features: Autoclave Sterilizable; Biocompatible; E-beam Sterilizable; Ethylene Oxide Sterilizable; Fatigue Resistant; Flame Retardant; Good Chemical Resistance; Good Dimensional Stability; Good Sterilizability; Heat Sterilizable; High Flow; High Heat Resistance; High Stiffness; High Strength; Radiation (Gamma) Resistant; Radiation Sterilizable; Radiotranslucent; Steam Resistant; Steam SterilizableUses: Aircraft Applications; Connectors; Dental Applications; Electrical/Electronic Applications; Film; Hospital Goods; Industrial Applications; Medical Devices; Medical/Healthcare Applications; Oil/Gas Applications; Pump Parts; Seals; Surgical InstrumentsInformation provided by Solvay Specialty Polymers.
Physical Properties Metric English Comments
Density 1.53 g/cc
0.0553 lb/in³
ASTM D792
Filler Content 30 %
30 %
Glass Fiber
Water Absorption 0.10 %

@Time 86400 sec
0.10 %

@Time 24.0 hour
ISO 62
Viscosity 350000 cP

@Shear Rate 1000 1/s,
Temperature 400 °C
350000 cP

@Shear Rate 1000 1/s,
Temperature 752 °F
Melt Viscosity; ASTM D3835
Linear Mold Shrinkage, Flow 0.0010 - 0.0030 cm/cm

@Thickness 3.18 mm
0.0010 - 0.0030 in/in

@Thickness 0.125 in
Linear Mold Shrinkage, Transverse 0.013 - 0.015 cm/cm

@Thickness 3.18 mm
0.013 - 0.015 in/in

@Thickness 0.125 in
ASTM D955
Melt Flow 14 g/10 min

@Load 2.16 kg,
Temperature 400 °C
14 g/10 min

@Load 4.76 lb,
Temperature 752 °F
ASTM D1238
Mechanical Properties Metric English Comments
Hardness, Rockwell M 105
105
ASTM D785
Tensile Strength 162 MPa
23500 psi
ASTM D638
Tensile Strength, Yield 174 MPa
25200 psi
5 mm/min, Type 1A; ISO 527-2
Elongation at Break 2.8 %
2.8 %
Type 1A, 5 mm/min; ISO 527-2
2.8 %
2.8 %
5 mm/min; ASTM D638
Tensile Modulus 10.8 GPa
1570 ksi
5 mm/min; ASTM D638
11.2 GPa
1620 ksi
ISO 527-2
Flexural Strength 239 MPa
34700 psi
ISO 178
260 MPa
37700 psi
ASTM D790
Flexural Modulus 10.5 GPa
1520 ksi
ASTM D790
10.6 GPa
1540 ksi
ISO 178
Compressive Strength 183 MPa
26500 psi
ASTM D695
Shear Strength 94.4 MPa
13700 psi
ASTM D732
Izod Impact, Notched 0.960 J/cm
1.80 ft-lb/in
ASTM D256
Izod Impact, Unnotched 8.50 J/cm
15.9 ft-lb/in
ASTM D256
Izod Impact, Notched (ISO) 11.0 kJ/m²
5.23 ft-lb/in²
ISO 180
Izod Impact, Unnotched (ISO) 62.0 kJ/m²
29.5 ft-lb/in²
ISO 180
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 19.0 µm/m-°C

@Temperature -50.0 - 50.0 °C
10.6 µin/in-°F

@Temperature -58.0 - 122 °F
1
Specific Heat Capacity 1.28 J/g-°C

@Temperature 50.0 °C
0.306 BTU/lb-°F

@Temperature 122 °F
ASTM C351
1.70 J/g-°C

@Temperature 200 °C
0.406 BTU/lb-°F

@Temperature 392 °F
ASTM C351
Thermal Conductivity 0.300 W/m-K
2.08 BTU-in/hr-ft²-°F
ASTM C177
Melting Point 343 °C
649 °F
ASTM D3418
Deflection Temperature at 1.8 MPa (264 psi) 315 °C
599 °F
Annealed; ASTM D648
Glass Transition Temp, Tg 147 °C
297 °F
DSC
Flammability, UL94 V-0

@Thickness 0.800 - 1.60 mm
V-0

@Thickness 0.0315 - 0.0630 in
Electrical Properties Metric English Comments
Volume Resistivity 3.80e+17 ohm-cm
3.80e+17 ohm-cm
ASTM D257
Surface Resistance >= 1.90e+17 ohm
>= 1.90e+17 ohm
ASTM D257
Dielectric Constant 3.49

@Frequency 1.00e+6 Hz
3.49

@Frequency 1.00e+6 Hz
ASTM D150
3.53

@Frequency 60.0 Hz
3.53

@Frequency 60.0 Hz
ASTM D150
3.53

@Frequency 1000 Hz
3.53

@Frequency 1000 Hz
ASTM D150
Dielectric Strength 16.0 kV/mm

@Thickness 3.00 mm
406 kV/in

@Thickness 0.118 in
ASTM D149
Dissipation Factor 0.0020

@Frequency 60.0 Hz
0.0020

@Frequency 60.0 Hz
ASTM D150
0.0020

@Frequency 1000 Hz
0.0020

@Frequency 1000 Hz
ASTM D150
0.0040

@Frequency 1.00e+6 Hz
0.0040

@Frequency 1.00e+6 Hz
ASTM D150
Processing Properties Metric English Comments
Rear Barrel Temperature 365 °C
689 °F
Middle Barrel Temperature 371 °C
700 °F
Front Barrel Temperature 377 °C
711 °F
Nozzle Temperature 382 °C
720 °F
Mold Temperature 177 - 204 °C
351 - 399 °F
Drying Temperature 150 °C

@Time 14400 sec
302 °F

@Time 4.00 hour
Descriptive Properties Value Comments
Agency Ratings FAA FAR 25.853a; ISO 10993; ISO 10993-Part 1
Availability Africa & Middle East
Asia Pacific
Europe
Latin America
North America
Color Light Beige
Form Pellets
Injection Rate Fast
Processing Technique Injection Molding; Machining; Profile Extrusion
RoHS Compliance RoHS Compliant
Screw Compression Ratio 2.5:1.0 to 3.5:1.0
Users viewing this material also viewed the following: