Rogers Corporation RT/duroid® 5880 Glass Microfiber Reinforced PTFE High Frequency Laminate

Category Polymer , Thermoplastic , Fluoropolymer , PTFE , Polytetrafluoroethylene (PTFE), Glass Filled, Molded
Manufacturer Rogers Corporation
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Rogers Corporation RT/duroid® 5880 Glass Microfiber Reinforced PTFE High Frequency Laminate.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
RT/duroid® 5870 and 5880 glass microfiber reinforced PTFE composites are designed for exacting stripline and microstrip circuit applications. Glass reinforcing microfibers are randomly oriented to maximize benefits of fiber reinforcement in the directions most valuable to circuit producers and in the final circuit applications.The dielectric constant of RT/duroid laminates is uniform from panel to panel and is constant over a wide frequency range. Its low dissipation factor extends the usefulness of RT/duroid 5870 and 5880 laminates to Ku-band and above.RT/duroid 5870 and 5880 laminates are easily cut, sheared and machined to shape. They are resistant to all solvents and reagents, hot or cold, normally used in etching printed circuits or in plating edges and holes.Available with a range of copper cladding options.Features:Lowest electrical loss for reinforced PTFE materialLow moisture absorptionIsotropicUniform electrical properties over frequencyExcellent chemical resistanceLead free process compatibleTypical Applications:Commercial Airline TelephonesMicrostrip and Stripline CircuitsMillimeter Wave ApplicationsMilitary Radar SystemsMissile Guidance SystemsPoint to Point Digital Radio AntennasInformation provided by Rogers Corporation.
Physical Properties Metric English Comments
Density 2.20 g/cc
0.0795 lb/in³
ASTM D792
Moisture Absorption at Equilibrium 0.020 %

@Thickness 1.57 mm
0.020 %

@Thickness 0.0620 in
D48/50; ASTM D570
Thickness 127 - 3180 microns
5.00 - 125 mil
Range of Thicknesses Available
Deformation 1.0 %

@Pressure 14.0 MPa,
Temperature 150 °C
1.0 %

@Pressure 2030 psi,
Temperature 302 °F
Z direction; 24 hrs; ASTM D621
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 18.0 MPa

@Temperature 100 °C
2610 psi

@Temperature 212 °F
Y direction, Condition A; ASTM D638
20.0 MPa

@Temperature 100 °C
2900 psi

@Temperature 212 °F
X direction, Condition A; ASTM D638
27.0 MPa

@Temperature 23.0 °C
3920 psi

@Temperature 73.4 °F
Y direction, Condition A; ASTM D638
29.0 MPa

@Temperature 23.0 °C
4210 psi

@Temperature 73.4 °F
X direction, Condition A; ASTM D638
Elongation at Break 4.9 %

@Temperature 23.0 °C
4.9 %

@Temperature 73.4 °F
Y direction, Condition A; ASTM D638
5.8 %

@Temperature 100 °C
5.8 %

@Temperature 212 °F
Y direction, Condition A; ASTM D638
6.0 %

@Temperature 23.0 °C
6.0 %

@Temperature 73.4 °F
X direction, Condition A; ASTM D638
7.2 %

@Temperature 100 °C
7.2 %

@Temperature 212 °F
X direction, Condition A; ASTM D638
Tensile Modulus 0.379 GPa

@Temperature 100 °C
55.0 ksi

@Temperature 212 °F
Y direction; ASTM D638
0.448 GPa

@Temperature 100 °C
65.0 ksi

@Temperature 212 °F
X direction; ASTM D638
0.862 GPa

@Temperature 23.0 °C
125 ksi

@Temperature 73.4 °F
Y direction; ASTM D638
1.08 GPa

@Temperature 23.0 °C
156 ksi

@Temperature 73.4 °F
X direction; ASTM D638
Compressive Strength 21.0 MPa

@Strain 7.80 %,
Temperature 100 °C
3050 psi

@Strain 7.80 %,
Temperature 212 °F
Y direction, Condition A; ASTM D695
22.0 MPa

@Strain 8.40 %,
Temperature 100 °C
3190 psi

@Strain 8.40 %,
Temperature 212 °F
X direction, Condition A; ASTM D695
27.0 MPa

@Strain 8.50 %,
Temperature 23.0 °C
3920 psi

@Strain 8.50 %,
Temperature 73.4 °F
X direction, Condition A; ASTM D695
29.0 MPa

@Strain 7.70 %,
Temperature 23.0 °C
4210 psi

@Strain 7.70 %,
Temperature 73.4 °F
Y direction, Condition A; ASTM D695
43.0 MPa

@Strain 17.6 %,
Temperature 100 °C
6240 psi

@Strain 17.6 %,
Temperature 212 °F
Z direction, Condition A; ASTM D695
52.0 MPa

@Strain 12.5 %,
Temperature 23.0 °C
7540 psi

@Strain 12.5 %,
Temperature 73.4 °F
Z direction, Condition A; ASTM D695
Compressive Modulus 0.500 GPa

@Temperature 100 °C
72.5 ksi

@Temperature 212 °F
X direction, Condition A; ASTM D695
0.500 GPa

@Temperature 100 °C
72.5 ksi

@Temperature 212 °F
Y direction, Condition A; ASTM D695
0.670 GPa

@Temperature 100 °C
97.2 ksi

@Temperature 212 °F
Z direction, Condition A; ASTM D695
0.710 GPa

@Temperature 23.0 °C
103 ksi

@Temperature 73.4 °F
X direction, Condition A; ASTM D695
0.710 GPa

@Temperature 23.0 °C
103 ksi

@Temperature 73.4 °F
Y direction, Condition A; ASTM D695
0.940 GPa

@Temperature 23.0 °C
136 ksi

@Temperature 73.4 °F
Z direction, Condition A; ASTM D695
Peel Strength 5.47 kN/m
31.2 pli
1 oz EDC foil; after solder float; IPC-TM-650 2.4.8
Thermal Properties Metric English Comments
CTE, linear 31.0 µm/m-°C

@Temperature 0.000 - 100 °C
17.2 µin/in-°F

@Temperature 32.0 - 212 °F
X-Direction; IPC-TM-650 2.4.41
48.0 µm/m-°C

@Temperature 0.000 - 100 °C
26.7 µin/in-°F

@Temperature 32.0 - 212 °F
Y-Direction; IPC-TM-650 2.4.41
237 µm/m-°C

@Temperature 0.000 - 100 °C
132 µin/in-°F

@Temperature 32.0 - 212 °F
Z-Direction; IPC-TM-650 2.4.41
Specific Heat Capacity 0.960 J/g-°C
0.229 BTU/lb-°F
calculated
Thermal Conductivity 0.200 W/m-K

@Temperature 80.0 °C
1.39 BTU-in/hr-ft²-°F

@Temperature 176 °F
Z direction; ASTM C518
Deflection Temperature at 1.8 MPa (264 psi) >= 260 °C
>= 500 °F
X, Y direction; ASTM D648
Decomposition Temperature 500 °C
932 °F
TGA; ASTM D3850
Flammability, UL94 V-0
V-0
Electrical Properties Metric English Comments
Volume Resistivity 2.00e+13 ohm-cm
2.00e+13 ohm-cm
Z direction; C96/35/90; ASTM D257
Surface Resistance 3.00e+13 ohm
3.00e+13 ohm
Z direction; C96/35/90; ASTM D257
Dielectric Constant 2.2

@Frequency 8.00e+9 - 4.00e+10 Hz
2.2

@Frequency 8.00e+9 - 4.00e+10 Hz
Design; Z direction; C24/23/50; IPC-TM-650 2.5.5.5
2.18 - 2.24

@Frequency 1.00e+10 Hz
2.18 - 2.24

@Frequency 1.00e+10 Hz
Process; Z direction; C24/23/50; IPC-TM-650 2.5.5.5
Dissipation Factor 0.00040

@Frequency 1.00e+6 Hz
0.00040

@Frequency 1.00e+6 Hz
Z direction; C24/23/50; IPC-TM-650 2.5.5.3
0.00090

@Frequency 1.00e+10 Hz
0.00090

@Frequency 1.00e+10 Hz
Z direction; C24/23/50; IPC-TM-650 2.5.5.5
Descriptive Properties Value Comments
Thermal Coefficient of Dielectric Constant -125 ppm/°C
IPC-TM-650 2.5.5.5; -50°C to 150°C