Category Polymer , Film , Thermoplastic , Polyethylene (PE) , MDPE , Linear Medium Density Polyethylene (LMDPE), Film
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Linear Medium Density Polyethylene (LMDPE), Film.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Linear Medium Density Polyethylene (LMDPE), Film". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 0.929 - 0.938 g/cc
0.0336 - 0.0339 lb/in³
Average value: 0.934 g/cc Grade Count:21
Moisture Vapor Transmission 0.230 - 0.350 cc-mm/m²-24hr-atm
0.584 - 0.889 cc-mil/100 in²-24hr-atm
Average value: 0.273 cc-mm/m²-24hr-atm Grade Count:6
Water Vapor Transmission 5.10 - 14.0 g/m²/day
0.328 - 0.902 g/100 in²/day
Average value: 7.49 g/m²/day Grade Count:6
Oxygen Transmission 78.0 - 133 cc-mm/m²-24hr-atm
198 - 338 cc-mil/100 in²-24hr-atm
Average value: 122 cc-mm/m²-24hr-atm Grade Count:5
Thickness 8.00 - 75.0 microns
0.315 - 2.95 mil
Average value: 31.5 microns Grade Count:8
Melt Flow 0.270 - 4.80 g/10 min
0.270 - 4.80 g/10 min
Average value: 2.15 g/10 min Grade Count:17
Mechanical Properties Metric English Comments
Hardness, Shore D 58.0 - 65.0
58.0 - 65.0
Average value: 60.2 Grade Count:6
Film Tensile Strength at Yield, MD 15.0 - 17.0 MPa
2180 - 2470 psi
Average value: 15.9 MPa Grade Count:16
Film Tensile Strength at Yield, TD 15.0 - 18.0 MPa
2180 - 2610 psi
Average value: 16.9 MPa Grade Count:16
Film Elongation at Break, MD 500 - 850 %
500 - 850 %
Average value: 663 % Grade Count:20
Film Elongation at Break, TD 750 - 1100 %
750 - 1100 %
Average value: 928 % Grade Count:16
Modulus of Elasticity 0.370 GPa
53.7 ksi
Average value: 0.370 GPa Grade Count:4
Secant Modulus, MD 0.280 - 0.450 GPa
40.6 - 65.3 ksi
Average value: 0.359 GPa Grade Count:15
Secant Modulus, TD 0.310 - 0.520 GPa
45.0 - 75.4 ksi
Average value: 0.417 GPa Grade Count:15
Coefficient of Friction 0.240 - 1.00
0.240 - 1.00
Average value: 0.523 Grade Count:14
Elmendorf Tear Strength, MD 0.815 - 4.00 g/micron
20.7 - 102 g/mil
Average value: 2.02 g/micron Grade Count:16
Elmendorf Tear Strength, TD 3.42 - 20.4 g/micron
86.9 - 518 g/mil
Average value: 11.2 g/micron Grade Count:16
Dart Drop 1.00 - 4.00 g/micron
25.4 - 102 g/mil
Average value: 1.96 g/micron Grade Count:9
Dart Drop Test 40.0 - 100 g
0.0882 - 0.221 lb
Average value: 71.1 g Grade Count:9
Seal Strength 1200 - 1400 g/25 mm
1200 - 1400 g/in
Average value: 1300 g/25 mm Grade Count:4
Film Tensile Strength at Break, MD 34.0 - 50.0 MPa
4930 - 7250 psi
Average value: 40.4 MPa Grade Count:20
Film Tensile Strength at Break, TD 25.0 - 44.0 MPa
3630 - 6380 psi
Average value: 34.7 MPa Grade Count:16
Thermal Properties Metric English Comments
Melting Point 124 - 128 °C
255 - 262 °F
Average value: 127 °C Grade Count:5
Vicat Softening Point 111 - 123 °C
232 - 253 °F
Average value: 117 °C Grade Count:12
Brittleness Temperature -75.0 - -70.0 °C
-103 - -94.0 °F
Average value: -70.6 °C Grade Count:9
Optical Properties Metric English Comments
Haze 3.00 - 20.0 %
3.00 - 20.0 %
Average value: 8.86 % Grade Count:18
Gloss 48.0 - 88.0 %
48.0 - 88.0 %
Average value: 72.8 % Grade Count:18
Transmission, Visible 90.0 %
90.0 %
Average value: 90.0 % Grade Count:4
Processing Properties Metric English Comments
Melt Temperature 210 - 290 °C
410 - 554 °F
Average value: 234 °C Grade Count:9