| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.05 g/cc | 1.05 g/cc | ASTM D792 |
| Maximum Moisture Content | 0.010 | 0.010 | Injection Molding |
| Linear Mold Shrinkage, Flow | 0.0040 - 0.0070 cm/cm <br>@Thickness 3.20 mm |
0.0040 - 0.0070 in/in <br>@Thickness 0.126 in |
ASTM D955 |
| Melt Flow | 40 g/10 min <br>@Load 10.0 kg,<br> Temperature 220 °C |
40 g/10 min <br>@Load 22.0 lb,<br> Temperature 428 °F |
ASTM D1238 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell R | 105 | 105 | ASTM D785 |
| Tensile Strength, Yield | 44.1 MPa <br>@Thickness 3.20 mm |
6400 psi <br>@Thickness 0.126 in |
50 mm/min; ASTM D638 |
| Elongation at Break | 40 % <br>@Thickness 3.20 mm |
40 % <br>@Thickness 0.126 in |
50 mm/min; ASTM D638 |
| Tensile Modulus | 1.96 GPa <br>@Thickness 3.20 mm |
284 ksi <br>@Thickness 0.126 in |
1 mm/min; ASTM D638 |
| Flexural Yield Strength | 68.6 MPa <br>@Thickness 3.20 mm |
9960 psi <br>@Thickness 0.126 in |
15 mm/min; ASTM D790 |
| Flexural Modulus | 2.30 GPa <br>@Thickness 3.20 mm |
334 ksi <br>@Thickness 0.126 in |
15 mm/min; ASTM D790 |
| Izod Impact, Notched | 2.84 J/cm <br>@Thickness 6.40 mm,<br> Temperature 23.0 °C |
5.33 ft-lb/in <br>@Thickness 0.252 in,<br> Temperature 73.4 °F |
ASTM D256 |
| 3.14 J/cm <br>@Thickness 3.20 mm,<br> Temperature 23.0 °C |
5.88 ft-lb/in <br>@Thickness 0.126 in,<br> Temperature 73.4 °F |
ASTM D256 | |
| Izod Impact, Unnotched | 0.981 J/cm <br>@Thickness 6.40 mm,<br> Temperature -30.0 °C |
1.84 ft-lb/in <br>@Thickness 0.252 in,<br> Temperature -22.0 °F |
ASTM D256 |
| 0.981 J/cm <br>@Thickness 3.20 mm,<br> Temperature -30.0 °C |
1.84 ft-lb/in <br>@Thickness 0.126 in,<br> Temperature -22.0 °F |
ASTM D256 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Deflection Temperature at 1.8 MPa (264 psi) | 87.0 °C <br>@Thickness 6.40 mm |
189 °F <br>@Thickness 0.252 in |
Unannealed; ASTM D648 |
| 92.0 °C <br>@Thickness 6.40 mm |
198 °F <br>@Thickness 0.252 in |
ASTM D648 | |
| Vicat Softening Point | 93.0 °C <br>@Load 5.00 kg |
199 °F <br>@Load 11.0 lb |
50°C/h; ASTM D1525 |
| UL RTI, Electrical | 60.0 °C <br>@Thickness >=1.50 mm |
140 °F <br>@Thickness >=0.0591 in |
UL 746B |
| 60.0 °C <br>@Thickness >=3.00 mm |
140 °F <br>@Thickness >=0.118 in |
||
| UL RTI, Mechanical with Impact | 60.0 °C <br>@Thickness >=1.50 mm |
140 °F <br>@Thickness >=0.0591 in |
UL 746B |
| 60.0 °C <br>@Thickness >=3.00 mm |
140 °F <br>@Thickness >=0.118 in |
||
| UL RTI, Mechanical without Impact | 60.0 °C <br>@Thickness >=1.50 mm |
140 °F <br>@Thickness >=0.0591 in |
UL 746B |
| 60.0 °C <br>@Thickness >=3.00 mm |
140 °F <br>@Thickness >=0.118 in |
||
| Flammability, UL94 | HB <br>@Thickness >=1.50 mm |
HB <br>@Thickness >=0.0591 in |
|
| HB <br>@Thickness >=3.00 mm |
HB <br>@Thickness >=0.118 in |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 1.00e+13 ohm-cm | 1.00e+13 ohm-cm | |
| Dielectric Strength | 34.0 kV/mm | 864 kV/in | |
| Arc Resistance | 60 - 120 sec | 60 - 120 sec | ASTM D495 |
| Comparative Tracking Index | 400 - 600 V | 400 - 600 V | Solution A; IEC 60112 |
| Hot Wire Ignition, HWI | 15 - 30 sec <br>@Thickness >=1.50 mm |
15 - 30 sec <br>@Thickness >=0.0591 in |
|
| 15 - 30 sec <br>@Thickness >=3.00 mm |
15 - 30 sec <br>@Thickness >=0.118 in |
||
| High Amp Arc Ignition, HAI | >= 120 arcs <br>@Thickness 1.50 mm |
>= 120 arcs <br>@Thickness 0.0591 in |
|
| >= 120 arcs <br>@Thickness 3.00 mm |
>= 120 arcs <br>@Thickness 0.118 in |
||
| High Voltage Arc-Tracking Rate, HVTR | 10.0 - 25.4 mm/min | 0.394 - 1.00 in/min |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Rear Barrel Temperature | 180 - 200 °C | 356 - 392 °F | Injection Molding |
| Middle Barrel Temperature | 190 - 210 °C | 374 - 410 °F | Injection Molding |
| Front Barrel Temperature | 200 - 220 °C | 392 - 428 °F | Injection Molding |
| Nozzle Temperature | 200 - 230 °C | 392 - 446 °F | Injection Molding |
| Melt Temperature | 210 - 240 °C | 410 - 464 °F | Injection Molding |
| Mold Temperature | 40.0 - 70.0 °C | 104 - 158 °F | Injection Molding |
| Drying Temperature | 80.0 °C | 176 °F | Injection Molding |
| Dry Time | 2.00 - 4.00 hour | 2.00 - 4.00 hour | Injection Molding |
| Back Pressure | 29.4 - 58.8 MPa | 4260 - 8530 psi | Injection Molding |
| Screw Speed | 30 - 60 rpm | 30 - 60 rpm | Injection Molding |