Overview of materials for Nylon 11 with 30% Glass Fiber Filler

Category Polymer , Thermoplastic , Nylon , Nylon 11 , Nylon 11 with 30% Glass Fiber Filler
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Nylon 11 with 30% Glass Fiber Filler.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 11 with 30% Glass Fiber Filler". Specific grades with glass content between 25% and 34% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.25 - 1.44 g/cc
0.0452 - 0.0520 lb/in³
Average value: 1.29 g/cc Grade Count:5
Water Absorption 0.100 - 1.30 %
0.100 - 1.30 %
Average value: 0.523 % Grade Count:3
Linear Mold Shrinkage 0.00100 - 0.00500 cm/cm
0.00100 - 0.00500 in/in
Average value: 0.00288 cm/cm Grade Count:3
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 86.2 - 115 MPa
12500 - 16700 psi
Average value: 101 MPa Grade Count:4
Elongation at Break 2.50 - 8.00 %
2.50 - 8.00 %
Average value: 5.30 % Grade Count:5
Modulus of Elasticity 6.55 - 8.00 GPa
950 - 1160 ksi
Average value: 7.31 GPa Grade Count:4
Flexural Yield Strength 124 - 179 MPa
18000 - 26000 psi
Average value: 145 MPa Grade Count:3
Flexural Modulus 5.52 - 6.07 GPa
800 - 880 ksi
Average value: 5.70 GPa Grade Count:3
Izod Impact, Notched 1.07 - 1.76 J/cm
2.00 - 3.30 ft-lb/in
Average value: 1.39 J/cm Grade Count:3
Charpy Impact Unnotched 8.39 - 8.39 J/cm²

@Temperature -30.0 - -30.0 °C
39.9 - 39.9 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 8.39 J/cm² Grade Count:1
Charpy Impact, Notched 1.20 - 1.20 J/cm²

@Temperature -30.0 - -30.0 °C
5.71 - 5.71 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 1.20 J/cm² Grade Count:1
Thermal Properties Metric English Comments
CTE, linear 50.0 - 54.0 µm/m-°C
27.8 - 30.0 µin/in-°F
Average value: 52.7 µm/m-°C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 180 - 192 °C
356 - 378 °F
Average value: 185 °C Grade Count:3
Deflection Temperature at 1.8 MPa (264 psi) 175 - 177 °C
347 - 350 °F
Average value: 176 °C Grade Count:3
Flammability, UL94 HB
HB
Grade Count:4
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+11 - 7.00e+13 ohm-cm
1.00e+11 - 7.00e+13 ohm-cm
Average value: 2.67e+13 ohm-cm Grade Count:3
Dielectric Strength 17.7 - 45.0 kV/mm
450 - 1140 kV/in
Average value: 27.5 kV/mm Grade Count:3