Material Notes:
Type: Isoplast® 300 is an engineering thermoplastic polyurethane resin.Appearance: Clear transparent pelletsApplication: Sheet extrusion, composite structures for industrial and consumer goods, injection molded parts.Features: The Isoplast 300U ETPU contains a special UV stabilizer package.Available in Americas, Europe, Middle East, Africa, India and Asia Information Provided by The Lubrizol Corporation
Physical Properties Metric English Comments
Specific Gravity 1.21 g/cc
1.21 g/cc
ISO 1183
Water Absorption 0.15 %

@Temperature 23.0 °C,
Time 86400 sec
0.15 %

@Temperature 73.4 °F,
Time 24.0 hour
ASTM D570
Linear Mold Shrinkage 0.050 - 0.060 cm/cm
0.050 - 0.060 in/in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Shore D 83

@Time 1.00 sec
83

@Time 0.000278 hour
ISO 868
Tensile Strength at Break 64.0 MPa
9280 psi
ISO 527-2/1A/5
Tensile Strength, Yield 63.0 MPa
9140 psi
ISO 527-2/1A/5
Elongation at Break 170 %
170 %
ISO 527-2/1A/5
Elongation at Yield 7.0 %
7.0 %
ISO 527-2/1A/5
Modulus of Elasticity 2.13 GPa
309 ksi
ISO 527-2/1A/1
Flexural Strength 85.0 MPa
12300 psi
ISO 178
Flexural Modulus 1.98 GPa
287 ksi
ISO 178
Izod Impact, Notched (ISO) 5.70 kJ/m²

@Temperature -30.0 °C
2.71 ft-lb/in²

@Temperature -22.0 °F
ISO 180/1A
8.20 kJ/m²

@Temperature 23.0 °C
3.90 ft-lb/in²

@Temperature 73.4 °F
ISO 180/1A
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 79.0 °C
174 °F
Method B; ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 69.0 °C
156 °F
Method A; ISO 75
Vicat Softening Point 96.0 °C
205 °F
ISO 360 (A50)
Glass Transition Temp, Tg 90.0 °C
194 °F
DSC
Optical Properties Metric English Comments
Yellow Index <= 15 %
<= 15 %
ASTM D1925
Transmission, Visible 92 %
92 %
ASTM D1003
Processing Properties Metric English Comments
Nozzle Temperature 225 - 235 °C
437 - 455 °F
Injection
Zone 1 205 - 215 °C
401 - 419 °F
Extrusion
205 - 215 °C
401 - 419 °F
Injection
Zone 2 210 - 220 °C
410 - 428 °F
Extrusion
215 - 225 °C
419 - 437 °F
Injection
Zone 3 215 - 225 °C
419 - 437 °F
Extrusion
220 - 230 °C
428 - 446 °F
Injection
Zone 4 220 - 230 °C
428 - 446 °F
Extrusion
225 - 235 °C
437 - 455 °F
Injection
Adapter Temperature 225 - 235 °C
437 - 455 °F
(5) Extrusion
Die Temperature 230 - 240 °C
446 - 464 °F
(6) Extrusion
230 - 240 °C
446 - 464 °F
(7) Tip, Extrusion
Mold Temperature 65.0 - 85.0 °C
149 - 185 °F
Injection