Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Nylon 6, Heat Stabilized

Category Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, Heat Stabilized
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Overview of materials for Nylon 6, Heat Stabilized.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Heat Stabilized". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.04 - 1.70 g/cc
0.0376 - 0.0614 lb/in³
Average value: 1.27 g/cc Grade Count:267
Filler Content 10.0 - 60.0 %
10.0 - 60.0 %
Average value: 28.7 % Grade Count:30
Water Absorption 0.200 - 10.0 %
0.200 - 10.0 %
Average value: 1.37 % Grade Count:154
Moisture Absorption at Equilibrium 0.250 - 2.80 %
0.250 - 2.80 %
Average value: 2.05 % Grade Count:32
Water Absorption at Saturation 3.90 - 10.0 %
3.90 - 10.0 %
Average value: 7.38 % Grade Count:38
Linear Mold Shrinkage 0.00100 - 0.0350 cm/cm
0.00100 - 0.0350 in/in
Average value: 0.00738 cm/cm Grade Count:232
Linear Mold Shrinkage, Transverse 0.00500 - 0.100 cm/cm
0.00500 - 0.100 in/in
Average value: 0.0118 cm/cm Grade Count:62
Melt Flow 1.00 - 100 g/10 min
1.00 - 100 g/10 min
Average value: 12.2 g/10 min Grade Count:19
Spiral Flow 35.0 - 107 cm
13.8 - 42.1 in
Average value: 77.5 cm Grade Count:11
Mechanical Properties Metric English Comments
Hardness, Rockwell L 113 - 123
113 - 123
Average value: 118 Grade Count:4
Hardness, Rockwell R 70.0 - 125
70.0 - 125
Average value: 114 Grade Count:122
Ball Indentation Hardness 75.0 - 290 MPa
10900 - 42100 psi
Average value: 160 MPa Grade Count:19
Tensile Strength, Ultimate 37.9 - 240 MPa
5500 - 34800 psi
Average value: 108 MPa Grade Count:88
Tensile Strength, Yield 29.0 - 234 MPa
4200 - 34000 psi
Average value: 104 MPa Grade Count:192
Elongation at Break 1.50 - 350 %
1.50 - 350 %
Average value: 36.2 % Grade Count:231
>= 100 %
<br>@Temperature 60.0 - 150 °C
>= 100 %
<br>@Temperature 140 - 302 °F
Average value: 100 % Grade Count:1
Elongation at Yield 2.00 - 200 %
2.00 - 200 %
Average value: 12.0 % Grade Count:25
Creep Strength 4.00 - 20.0 MPa
580 - 2900 psi
Average value: 11.9 MPa Grade Count:10
Modulus of Elasticity 0.470 - 21.0 GPa
68.2 - 3050 ksi
Average value: 5.79 GPa Grade Count:83
0.300 - 0.550 GPa
<br>@Temperature 60.0 - 150 °C
43.5 - 79.8 ksi
<br>@Temperature 140 - 302 °F
Average value: 0.379 GPa Grade Count:1
Flexural Yield Strength 9.65 - 370 MPa
1400 - 53700 psi
Average value: 151 MPa Grade Count:233
Flexural Modulus 0.469 - 20.0 GPa
68.0 - 2900 ksi
Average value: 4.97 GPa Grade Count:236
Compressive Yield Strength 29.0 - 147 MPa
4210 - 21300 psi
Average value: 66.6 MPa Grade Count:12
Poissons Ratio 0.350
0.350
Average value: 0.350 Grade Count:4
Izod Impact, Notched 0.374 - 5340 J/cm
0.700 - 10000 ft-lb/in
Average value: 1.46 J/cm Grade Count:180
0.186865 - 5338.47 J/cm
<br>@Temperature -40.0 - -20.0 °C
0.350075 - 10001.1 ft-lb/in
<br>@Temperature -40.0 - -4.00 °F
Average value: 1.56 J/cm Grade Count:19
0.186865 - 5338.47 J/cm
<br>@Thickness 1.57 - 3.17 mm
0.350075 - 10001.1 ft-lb/in
<br>@Thickness 0.0618 - 0.125 in
Average value: 1.56 J/cm Grade Count:19
Izod Impact, Unnotched 3.20 - 5340 J/cm
6.00 - 10000 ft-lb/in
Average value: 9.89 J/cm Grade Count:45
Izod Impact, Notched (ISO) 2.50 - 100000 kJ/m²
1.19 - 47600 ft-lb/in²
Average value: 14.6 kJ/m² Grade Count:33
3.00 - 20.0 kJ/m²
<br>@Temperature -40.0 - -20.0 °C
1.43 - 9.52 ft-lb/in²
<br>@Temperature -40.0 - -4.00 °F
Average value: 10.0 kJ/m² Grade Count:19
Izod Impact, Unnotched (ISO) 30.0 - 110 kJ/m²
14.3 - 52.3 ft-lb/in²
Average value: 67.0 kJ/m² Grade Count:12
30.0 - 100 kJ/m²
<br>@Temperature -30.0 - -30.0 °C
14.3 - 47.6 ft-lb/in²
<br>@Temperature -22.0 - -22.0 °F
Average value: 57.0 kJ/m² Grade Count:12
Charpy Impact Unnotched 2.00 J/cm² - NB
9.52 ft-lb/in² - NB
Average value: 7.53 J/cm² Grade Count:56
1.50 J/cm² - NB
<br>@Temperature -30.0 - -20.0 °C
7.14 ft-lb/in² - NB
<br>@Temperature -22.0 - -4.00 °F
Average value: 5.64 J/cm² Grade Count:42
Charpy Impact, Notched 0.150 - 13.0 J/cm²
0.714 - 61.9 ft-lb/in²
Average value: 1.44 J/cm² Grade Count:56
0.150 - 2.00 J/cm²
<br>@Temperature -30.0 - -20.0 °C
0.714 - 9.52 ft-lb/in²
<br>@Temperature -22.0 - -4.00 °F
Average value: 0.863 J/cm² Grade Count:43
Gardner Impact 36.2 J
26.7 ft-lb
Average value: 36.2 J Grade Count:3
Puncture Energy 64.0 - 64.0 J
<br>@Temperature -30.0 - -30.0 °C
47.2 - 47.2 ft-lb
<br>@Temperature -22.0 - -22.0 °F
Average value: 64.0 J Grade Count:1
Coefficient of Friction 0.0400 - 0.390
0.0400 - 0.390
Average value: 0.204 Grade Count:14
Tear Strength Test 0.150 - 0.250
0.150 - 0.250
Average value: 0.190 Grade Count:10
K Factor (Wear Factor) 9.00e-11 - 0.440
9.00e-11 - 0.440
Average value: 0.0400 Grade Count:11
Thermal Properties Metric English Comments
CTE, linear 7.20 - 150 µm/m-°C
4.00 - 83.3 µin/in-°F
Average value: 48.9 µm/m-°C Grade Count:143
CTE, linear, Transverse to Flow 80.0 - 150 µm/m-°C
44.4 - 83.3 µin/in-°F
Average value: 97.0 µm/m-°C Grade Count:12
Specific Heat Capacity 1.67 J/g-°C
0.399 BTU/lb-°F
Average value: 1.67 J/g-°C Grade Count:10
Thermal Conductivity 0.250 - 0.330 W/m-K
1.74 - 2.29 BTU-in/hr-ft²-°F
Average value: 0.265 W/m-K Grade Count:13
Melting Point 215 - 260 °C
419 - 500 °F
Average value: 221 °C Grade Count:102
Maximum Service Temperature, Air 85.0 - 190 °C
185 - 374 °F
Average value: 147 °C Grade Count:14
Deflection Temperature at 0.46 MPa (66 psi) 95.0 - 227 °C
203 - 440 °F
Average value: 199 °C Grade Count:172
Deflection Temperature at 1.8 MPa (264 psi) 49.0 - 250 °C
120 - 482 °F
Average value: 144 °C Grade Count:231
Deflection Temperature at 8.0 MPa 55.0 - 190 °C
131 - 374 °F
Average value: 142 °C Grade Count:5
Electrical Properties Metric English Comments
Electrical Resistivity 1.00 - 1.00e+16 ohm-cm
1.00 - 1.00e+16 ohm-cm
Average value: 8.55e+14 ohm-cm Grade Count:156
Surface Resistance 1.00 - 1.00e+16 ohm
1.00 - 1.00e+16 ohm
Average value: 9.02e+14 ohm Grade Count:59
Dielectric Constant 3.00 - 4.00
3.00 - 4.00
Average value: 3.55 Grade Count:20
Dielectric Strength 15.4 - 80.0 kV/mm
390 - 2030 kV/in
Average value: 20.4 kV/mm Grade Count:137
Dissipation Factor 0.00500 - 0.0180
0.00500 - 0.0180
Average value: 0.0114 Grade Count:7
Dielectric Loss Index 0.0300
0.0300
Average value: 0.0300 Grade Count:10
Comparative Tracking Index 350 - 600 V
350 - 600 V
Average value: 554 V Grade Count:38
Copyright © lookpolymers.com All Rights Reserved