Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Gardner Impact | >= 36.2 J @Temperature -30.0 °C |
>= 26.7 ft-lb @Temperature -22.0 °F |
ASTM D5420 |
Network Polymers Softflex® 0250 Description: Softflex® Thermoplastic Elastomer AlloyInformation provided by Network Polymers Inc. |
|||
Gardner Impact | >= 36.2 J @Temperature -30.0 °C |
>= 26.7 ft-lb @Temperature -22.0 °F |
ASTM D5420 |
Network Polymers Softflex® 0470 Description: Softflex® Thermoplastic Elastomer AlloyInformation provided by Network Polymers Inc. |
|||
Gardner Impact | >= 36.2 J | >= 26.7 ft-lb | ASTM D3029 |
Polymer Resources ABS-FR1 ABS, Flame Retardant Process: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples. Information provided by Polymer Resources Corporation. |
|||
Gardner Impact | >= 36.2 J | >= 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC/ABS-FR1-[color]-3 PC Blend, Flame Retardant, Standard Flow, UV Stabilized Process: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples. Information provided by Polymer Resources Corporation. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC/TP-FR3 Flame Retardant PC/Polyester Alloy Flame Retardant, High Impact, Excellent Chemical ResistanceFeatures: • Flame Retardant • Impact Modified • Self Extinguishing • Good Chemical ResistanceProcess: Injection MoldingNotes: All p.. |
|||
Gardner Impact | >= 36.2 J | >= 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC/TP-GP1-[color]-3 PC Polyester, High Impact, Good Chemical Resistance, UV-stabilized Process: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples. Information provided by Polymer Resources Corporation. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-FR2-D-[color]-3 Polycarbonate, Improved Flame Retardant, Medium Flow, UV-stabilized Polycarbonate, Improved Flame Retardant, Medium Flow, UV-stabilizedProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test sampl.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP1-[color]-LF Polycarbonate, General Purpose, Food Contact Polycarbonate, General Purpose, Low FlowFeatures: • Food Contact AcceptableProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, .. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP1-D-[color]-1 Polycarbonate, General Purpose, Low Flow with Mold Release Polycarbonate, General Purpose, Low Flow with Mold ReleaseProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.Inform.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP1-D-[color]-6 Polycarbonate, FDA-compliant Feedstocks, Low Flow with Mold Release Polycarbonate, FDA-compliant Feedstocks, Low Flow with Mold ReleaseProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test sampl.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP2-D Polycarbonate, General Purpose, Medium Flow Polycarbonate, General Purpose, Medium FlowFeatures: • Ultra High Impact Resistance • Self ExtinguishingProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP3-D-[color]-5 Polycarbonate, FDA-compliant Feedstocks, High Flow Polycarbonate, FDA-compliant Feedstocks, High FlowProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.Information pr.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP3-D-[color]-6 Polycarbonate, FDA-compliant Feedstocks, High Flow with Mold Release Polycarbonate, FDA-compliant Feedstocks, High Flow with Mold ReleaseProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samp.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP3-TFE5 Polycarbonate, 5% PTFE, High Flow, Wear Resistant Polycarbonate, General Purpose, High Flow, Wear ResistantProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.Informa.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP4-[color]-5 Polycarbonate, FDA-compliant Feedstocks, Easy Flow Polycarbonate, FDA-compliant Feedstocks, Easy FlowProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.Information pr.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP4-[color]-6 Polycarbonate, FDA-compliant Feedstocks, Easy Flow with Mold Release Polycarbonate, FDA-compliant Feedstocks, Easy Flow with Mold ReleaseProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samp.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-IM2-UV Polycarbonate, Impact Modified, Medium Flow, UV-stabilized Polycarbonate, Impact Modified, Medium Flow, UV-stabilizedProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.Inform.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-UV1-D Polycarbonate, UV-stabilized, Low Flow Polycarbonate, UV-stabilized, Low FlowProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.Information provided by Po.. |
|||
Gardner Impact | >= 36.2 J | >= 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC/TP-GP2 PC Polyester, High Impact, Excellent Chemical Resistance
(Unverified Data**)& Process: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples. Information provided by Polymer Resources Corporation. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources NY6-GP2-[color]-H General Purpose Nylon 6, Nucleated, Heat Stabilized General Purpose Nylon 6, Nucleated, Heat StabilizedProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples. Nylon grades.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC/ABS-GP1-[color]-EP General Purpose PC/ABS Alloy, Electroplating Grade PC/ABS Alloy, General Purpose, Electroplating GradeProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.Information p.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-FD4 Polycarbonate, FDA-compliant Feedstocks, Easy Flow, Gamma Resistant Polycarbonate, FDA-compliant Feedstocks, Easy Flow, Gamma ResistantProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test sampl.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | ASTM D3029 |
Polymer Resources PC-GP3-D-[color]-1 Polycarbonate, General Purpose, High Flow with Mold Release Polycarbonate, General Purpose, High Flow with Mold ReleaseProcess: Injection MoldingNotes: All physical, mechanical and thermal testing conducted on 1/8-inch thick, un-pigmented, test samples.Infor.. |
|||
Gardner Impact | 36.2 J @Temperature -30.0 °C |
26.7 ft-lb @Temperature -22.0 °F |
ASTM D3029 |
DuPont Bexloy® AXW507NC010 Modified Ionomer Resin
(discontinued **) A modified ionomer resin engineered for injection molded exterior automotive applications.Availability: North AmericaInformation provided by DuPont. |
|||
Gardner Impact | 36.2 J @Temperature 23.0 °C |
26.7 ft-lb @Temperature 73.4 °F |
ASTM D 5420 |
Shakespeare Isocorâ„¢ SVP6105 medium viscosity PA-610 Isocorâ„¢ 6105 is a medium viscosity PA-610. This resin is specifically suited for applications requiring low moisture absorption and greater dimensional stability. Isocorâ„¢ 6105 is also .. |
|||
Gardner Impact | 36.2 J @Temperature 23.0 °C |
26.7 ft-lb @Temperature 73.4 °F |
1/2" R Tup125 mil |
Axiall SP-6340 Rigid PVC, Molding Georgia Gulf SP-6340 is a rigid vinyl injection molding compound designed for fittings and parts of similar confiation where maximum burst strength is required. Georgia Gulf 6340 is ideally suited .. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | Average value: 36.2 J Grade Count:3 |
Overview of materials for Nylon 6, Heat Stabilized This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Heat Stabilized". Each property range of values reported is minimum and maximum values of appro.. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | Average value: 36.2 J Grade Count:7 |
Overview of materials for Polycarbonate, PTFE Filled This property data is a summary of similar materials in the MatWeb database for the category "Polycarbonate, PTFE Filled". Each property range of values reported is minimum and maximum values of app.. |
|||
Gardner Impact | >= 36.2 J | >= 26.7 ft-lb | CP-TM-11 |
PolyOne Elastamax HTE 2101-1002 Polyurethane Alloy
(discontinued **) This is an extrusion grade polyurethane alloy. Physical Form: Pellet. Standard Color: Off white, opaque.Information provided by M. A. Hanna. M. A. Hanna and Geon merged to form PolyOne in 2000. .. |
|||
Gardner Impact | 36.2 J | 26.7 ft-lb | Average value: 36.2 J Grade Count:5 |
Overview of materials for Nylon 6, Unreinforced This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Unreinforced". Each property range of values reported is minimum and maximum values of appropri.. |