| Category | Polymer , Thermoplastic , Polyester, TP , Polybutylene Terephthalate (PBT) , Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled |
| Manufacturer | LG Chemical |
| Trade Name | Lupox® |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | LG Chemical Lupox® GP2056F PBT+GF5%.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.47 g/cc | 1.47 g/cc | ASTM D792 |
| Maximum Moisture Content | 0.020 | 0.020 | Injection Molding |
| Linear Mold Shrinkage, Flow | 0.0050 - 0.012 cm/cm @Thickness 3.20 mm |
0.0050 - 0.012 in/in @Thickness 0.126 in |
ASTM D955 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 58.8 MPa @Thickness 3.20 mm |
8530 psi @Thickness 0.126 in |
50mm/min; ASTM D638 |
| Elongation at Break | 4.0 % @Thickness 3.20 mm |
4.0 % @Thickness 0.126 in |
5mm/min; ASTM D638 |
| Flexural Yield Strength | 98.1 MPa @Thickness 3.20 mm |
14200 psi @Thickness 0.126 in |
1.3mm/min; ASTM D790 |
| Flexural Modulus | 3.73 GPa @Thickness 3.20 mm |
540 ksi @Thickness 0.126 in |
1.3mm/min; ASTM D790 |
| Izod Impact, Notched | 0.294 J/cm @Thickness 3.20 mm, Temperature 23.0 °C |
0.551 ft-lb/in @Thickness 0.126 in, Temperature 73.4 °F |
ASTM D256 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Melting Point | 225 °C | 437 °F | @ Break; ASTM D3418 |
| Deflection Temperature at 0.46 MPa (66 psi) | 190 °C @Thickness 6.40 mm |
374 °F @Thickness 0.252 in |
Unannealed; ASTM D648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 130 °C @Thickness 6.40 mm |
266 °F @Thickness 0.252 in |
Unannealed; ASTM D648 |
| UL RTI, Electrical | 130 °C @Thickness >=0.710 mm |
266 °F @Thickness >=0.0280 in |
|
| 130 °C @Thickness >=1.50 mm |
266 °F @Thickness >=0.0591 in |
||
| 130 °C @Thickness >=3.00 mm |
266 °F @Thickness >=0.118 in |
||
| UL RTI, Mechanical with Impact | 130 °C @Thickness >=0.710 mm |
266 °F @Thickness >=0.0280 in |
|
| 130 °C @Thickness >=1.50 mm |
266 °F @Thickness >=0.0591 in |
||
| 130 °C @Thickness >=3.00 mm |
266 °F @Thickness >=0.118 in |
||
| UL RTI, Mechanical without Impact | 140 °C @Thickness >=0.710 mm |
284 °F @Thickness >=0.0280 in |
|
| 140 °C @Thickness >=1.50 mm |
284 °F @Thickness >=0.0591 in |
||
| 140 °C @Thickness >=3.00 mm |
284 °F @Thickness >=0.118 in |
||
| Flammability, UL94 | V-0 @Thickness >=0.710 mm |
V-0 @Thickness >=0.0280 in |
|
| V-0 @Thickness >=1.50 mm |
V-0 @Thickness >=0.0591 in |
||
| V-0 @Thickness >=3.00 mm |
V-0 @Thickness >=0.118 in |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 1.00e+16 ohm-cm | 1.00e+16 ohm-cm | ASTM D257 |
| Dielectric Strength | 23.0 kV/mm @Thickness 1.00 mm |
584 kV/in @Thickness 0.0394 in |
ASTM D149 |
| Arc Resistance | 60 - 120 sec | 60 - 120 sec | ASTM D495 |
| Comparative Tracking Index | 175 V | 175 V | Solution A; IEC 60112 |
| Hot Wire Ignition, HWI | 7.0 - 15 sec @Thickness >=0.710 mm |
7.0 - 15 sec @Thickness >=0.0280 in |
|
| 15 - 30 sec @Thickness >=1.50 mm |
15 - 30 sec @Thickness >=0.0591 in |
||
| 15 - 30 sec @Thickness >=3.00 mm |
15 - 30 sec @Thickness >=0.118 in |
||
| High Amp Arc Ignition, HAI | 0.00 - 15 arcs @Thickness 0.710 mm |
0.00 - 15 arcs @Thickness 0.0280 in |
|
| 60 - 120 arcs @Thickness 1.50 mm |
60 - 120 arcs @Thickness 0.0591 in |
||
| >= 120 arcs @Thickness 3.00 mm |
>= 120 arcs @Thickness 0.118 in |
||
| High Voltage Arc-Tracking Rate, HVTR | 80.0 - 150 mm/min | 3.15 - 5.91 in/min |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Rear Barrel Temperature | 235 - 250 °C | 455 - 482 °F | Injection Molding |
| Middle Barrel Temperature | 240 - 250 °C | 464 - 482 °F | Injection Molding |
| Front Barrel Temperature | 245 - 255 °C | 473 - 491 °F | Injection Molding |
| Nozzle Temperature | 245 - 255 °C | 473 - 491 °F | Injection Molding |
| Melt Temperature | 245 - 255 °C | 473 - 491 °F | Injection Molding |
| Mold Temperature | 60.0 - 100 °C | 140 - 212 °F | Injection Molding |
| Drying Temperature | 130 °C | 266 °F | Injection Molding |
| Dry Time | 4.00 - 5.00 hour | 4.00 - 5.00 hour | Injection Molding |