Material Notes:
Low viscosity, RT cure. Easy processing.Processing: 100/10 pbw; Potlife: 2.5 h/20°C (68°F), 30 min/40°C (105°F), 15 min/60°C (140°F); mix at RT; cures in: 24 h/20°C (68°F), 2-3 h/60°C (140°F), 15 min/100°C (212°F).Applications: Laminating, small parts, and potting.
Physical Properties Metric English Comments
Density 1.18 g/cc
0.0426 lb/in³
Water Absorption 0.30 - 0.50 %
0.30 - 0.50 %
(60x10X4 mm bar) after 10 days at 20°C (77°F)
0.70 - 1.0 %
0.70 - 1.0 %
(60x10X4 mm bar) after 1 hour at 100°C (212°F)
Viscosity 1600 - 2000 cP
1600 - 2000 cP
Vapor Pressure <= 0.0000133 bar

@Temperature 20.0 °C
<= 0.0100 torr

@Temperature 68.0 °F
AboCure
<= 0.00133 bar

@Temperature 100 °C
<= 1.00 torr

@Temperature 212 °F
AboCast
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 65.5 MPa
9500 psi
Modulus of Elasticity 3.447 GPa
500.0 ksi
Flexural Yield Strength 96.53 MPa
14000 psi
Compressive Yield Strength 103.4 MPa
15000 psi
Thermal Properties Metric English Comments
CTE, linear 90.0 - 95.0 µm/m-°C

@Temperature 20.0 °C
50.0 - 52.8 µin/in-°F

@Temperature 68.0 °F
Thermal Conductivity 0.150 - 0.170 W/m-K
1.04 - 1.18 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 55.0 °C
131 °F
Deflection temperature; load unknown.
Electrical Properties Metric English Comments
Electrical Resistivity >= 1.50e+16 ohm-cm
>= 1.50e+16 ohm-cm
Dielectric Constant 3.6 - 3.8

@Frequency 1e+6 Hz
3.6 - 3.8

@Frequency 1e+6 Hz
3.8 - 4.0

@Frequency 1000 Hz
3.8 - 4.0

@Frequency 1000 Hz
3.9 - 4.1

@Frequency 50 Hz
3.9 - 4.1

@Frequency 50 Hz
Dielectric Strength 15.7 - 19.7 kV/mm

@Thickness 3.17 mm
400 - 500 kV/in

@Thickness 0.125 in
Short time value
Dissipation Factor 0.010 - 0.020

@Frequency 50 Hz
0.010 - 0.020

@Frequency 50 Hz
0.010 - 0.020

@Frequency 1000 Hz
0.010 - 0.020

@Frequency 1000 Hz
0.020 - 0.030

@Frequency 1e+6 Hz
0.020 - 0.030

@Frequency 1e+6 Hz
Processing Properties Metric English Comments
Processing Temperature 25.0 °C
77.0 °F
Pot Life 15.0 min

@Temperature 60.0 °C
15.0 min

@Temperature 140 °F
30.0 min

@Temperature 40.0 °C
30.0 min

@Temperature 104 °F
150 min

@Temperature 20.0 °C
150 min

@Temperature 68.0 °F