Category | Polymer , Thermoplastic , Polycarbonate (PC) |
Manufacturer | SABIC Innovative Plastics (GE Plastics) |
Trade Name | Lexan® |
Port | Ningbo port,China |
Trade Terms | FOB, CFR, CIF |
Payment Terms | L/C, T/T, Western Union |
Download PDF | SABIC Innovative Plastics Lexan® EXL6414 PC (Asia Pacific).pdf ![]() |
Price | EMAIL US sales@lookpolymers.com |
Physical Properties | Metric | English | Comments |
---|---|---|---|
Specific Gravity | 1.19 g/cc | 1.19 g/cc | ASTM D792 |
Density | 1.18 g/cc | 0.0426 lb/in³ | ISO 1183 |
Moisture Absorption | 0.150 % | 0.150 % | 23°C / 50% RH; ISO 62 |
Water Absorption at Saturation | 0.35 % | 0.35 % | ISO 62 |
Linear Mold Shrinkage, Flow | 0.0040 - 0.0080 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0080 in/in @Thickness 0.126 in |
SABIC Method |
Linear Mold Shrinkage, Transverse | 0.0040 - 0.0080 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0080 in/in @Thickness 0.126 in |
SABIC Method |
Melt Flow | 8.0 g/10 min @Load 1.20 kg, Temperature 300 °C |
8.0 g/10 min @Load 2.65 lb, Temperature 572 °F |
ASTM D1238 |
Melt Index of Compound | 7.0 g/10 min @Load 1.20 kg, Temperature 300 °C |
7.0 g/10 min @Load 2.65 lb, Temperature 572 °F |
MVR [cm^3/10 min]; ISO 1133 |
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Tensile Strength at Break | 58.0 MPa | 8410 psi | 50 mm/min; ISO 527 |
59.0 MPa | 8560 psi | Type I, 50 mm/min; ASTM D638 | |
Tensile Strength, Yield | 54.0 MPa | 7830 psi | 50 mm/min; ISO 527 |
55.0 MPa | 7980 psi | Type I, 50 mm/min; ASTM D638 | |
Elongation at Break | 88 % | 88 % | 50 mm/min; ISO 527 |
100 % | 100 % | Type I, 50 mm/min; ASTM D638 | |
Elongation at Yield | 5.5 % | 5.5 % | Type I, 50 mm/min; ASTM D638 |
6.0 % | 6.0 % | 50 mm/min; ISO 527 | |
Tensile Modulus | 1.72 GPa | 249 ksi | 50 mm/min; ASTM D638 |
2.27 GPa | 329 ksi | 1 mm/min; ISO 527 | |
Flexural Yield Strength | 79.0 MPa | 11500 psi | 1.3 mm/min, 50 mm span; ASTM D790 |
85.0 MPa | 12300 psi | 2 mm/min; ISO 178 | |
Flexural Modulus | 1.99 GPa | 289 ksi | 1.3 mm/min, 50 mm span; ASTM D790 |
2.09 GPa | 303 ksi | 2 mm/min; ISO 178 | |
Izod Impact, Notched | 8.01 J/cm | 15.0 ft-lb/in | ASTM D256 |
6.94 J/cm @Temperature -30.0 °C |
13.0 ft-lb/in @Temperature -22.0 °F |
ASTM D256 | |
Izod Impact, Unnotched | 32.04 J/cm | 60.02 ft-lb/in | ASTM D4812 |
Izod Impact, Notched (ISO) | 70.0 kJ/m² | 33.3 ft-lb/in² | 80*10*3; ISO 180/1A |
60.0 kJ/m² @Temperature -30.0 °C |
28.6 ft-lb/in² @Temperature -22.0 °F |
80*10*3; ISO 180/1A | |
Izod Impact, Unnotched (ISO) | NB | NB | 80*10*3; ISO 180/1U |
NB @Temperature -30.0 °C |
NB @Temperature -22.0 °F |
80*10*3; ISO 180/1U | |
Charpy Impact Unnotched | NB | NB | Edgew 80*10*3 sp=62mm; ISO 179/1eU |
NB @Temperature -30.0 °C |
NB @Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eU | |
Charpy Impact, Notched | 7.00 J/cm² | 33.3 ft-lb/in² | Edgew 80*10*3 sp=62mm; ISO 179/1eA |
6.00 J/cm² @Temperature -30.0 °C |
28.6 ft-lb/in² @Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eA | |
Dart Drop, Total Energy | 61.0 J @Temperature -30.0 °C |
45.0 ft-lb @Temperature -22.0 °F |
ASTM D3763 |
62.0 J @Temperature 23.0 °C |
45.7 ft-lb @Temperature 73.4 °F |
ASTM D3763 |
Thermal Properties | Metric | English | Comments |
---|---|---|---|
CTE, linear, Parallel to Flow | 69.0 µm/m-°C @Temperature 23.0 - 80.0 °C |
38.3 µin/in-°F @Temperature 73.4 - 176 °F |
ISO 11359-2 |
70.2 µm/m-°C @Temperature -40.0 - 40.0 °C |
39.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 | |
CTE, linear, Transverse to Flow | 72.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
40.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
73.0 µm/m-°C @Temperature 23.0 - 80.0 °C |
40.6 µin/in-°F @Temperature 73.4 - 176 °F |
ISO 11359-2 | |
Deflection Temperature at 0.46 MPa (66 psi) | 136 °C | 277 °F | Edgew 120*10*4 sp=100mm; ISO 75/Be |
136 °C @Thickness 3.20 mm |
277 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
Deflection Temperature at 1.8 MPa (264 psi) | 122 °C | 252 °F | Edgew 120*10*4 sp=100mm; ISO 75/Ae |
122 °C @Thickness 3.20 mm |
252 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
Vicat Softening Point | 140 °C | 284 °F | Rate B/120; ISO 306 |
141 °C | 286 °F | Rate B/50; ASTM D1525 | |
141 °C | 286 °F | Rate B/50; ISO 306 | |
UL RTI, Electrical | 80.0 °C | 176 °F | UL 746B |
UL RTI, Mechanical with Impact | 80.0 °C | 176 °F | UL 746B |
UL RTI, Mechanical without Impact | 80.0 °C | 176 °F | UL 746B |
Flammability, UL94 | HB @Thickness 1.47 mm |
HB @Thickness 0.0579 in |
UL 94 |
Electrical Properties | Metric | English | Comments |
---|---|---|---|
Volume Resistivity | 1.70e+17 ohm-cm | 1.70e+17 ohm-cm | IEC 60093 |
Surface Resistance | 4.10e+17 ohm | 4.10e+17 ohm | ROA; IEC 60093 |
Dielectric Constant | 2.6 @Frequency 1.00e+6 Hz |
2.6 @Frequency 1.00e+6 Hz |
IEC 60250 |
Dielectric Strength | 18.0 kV/mm @Thickness 3.20 mm |
457 kV/in @Thickness 0.126 in |
in oil; IEC 60243-1 |
Dissipation Factor | 0.0094 @Frequency 1.00e+6 Hz |
0.0094 @Frequency 1.00e+6 Hz |
IEC 60250 |
Arc Resistance | 120 - 180 sec | 120 - 180 sec | Tungsten; ASTM D495 |
Comparative Tracking Index | 175 - 250 V | 175 - 250 V | UL 746A |
Hot Wire Ignition, HWI | 30 - 60 sec | 30 - 60 sec | UL 746A |
High Amp Arc Ignition, HAI | >= 120 arcs | >= 120 arcs | UL 746A |
High Voltage Arc-Tracking Rate, HVTR | 80.0 - 150 mm/min | 3.15 - 5.91 in/min | UL 746A |
Descriptive Properties | Value | Comments |
---|---|---|
Ball Pressure Test, 125°C +/- 2°C | PASSES | IEC 60695-10-2 |