| Category | Polymer , Thermoplastic , ABS Polymer , Polycarbonate/ABS Alloy, Unreinforced , Polycarbonate (PC) |
| Manufacturer | SABIC Innovative Plastics (GE Plastics) |
| Trade Name | Cycoloy® |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | SABIC Innovative Plastics Cycoloy® CM6140 PC+ABS (Asia Pacific).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.26 g/cc | 1.26 g/cc | ASTM D792 |
| Density | 1.25 g/cc | 0.0452 lb/in³ | ISO 1183 |
| Water Absorption | 0.10 % <br>@Time 86400 sec |
0.10 % <br>@Time 24.0 hour |
ASTM D570 |
| Moisture Absorption | 0.0100 % | 0.0100 % | 50% RH, 24 hrs; ASTM D570 |
| 0.0100 % | 0.0100 % | 23°C / 50% RH; ISO 62 | |
| Water Absorption at Saturation | 0.090 % | 0.090 % | ISO 62 |
| Linear Mold Shrinkage, Flow | 0.0030 - 0.0050 cm/cm <br>@Thickness 3.20 mm |
0.0030 - 0.0050 in/in <br>@Thickness 0.126 in |
SABIC Method |
| Linear Mold Shrinkage, Transverse | 0.0040 - 0.0060 cm/cm <br>@Thickness 3.20 mm |
0.0040 - 0.0060 in/in <br>@Thickness 0.126 in |
SABIC Method |
| Melt Flow | 17.5 g/10 min <br>@Load 2.16 kg,<br> Temperature 260 °C |
17.5 g/10 min <br>@Load 4.76 lb,<br> Temperature 500 °F |
ASTM D1238 |
| Melt Index of Compound | 14 g/10 min <br>@Load 5.00 kg,<br> Temperature 220 °C |
14 g/10 min <br>@Load 11.0 lb,<br> Temperature 428 °F |
MVR [cm^3/10 min]; ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 50.0 MPa | 7250 psi | Type I, 5 mm/min; ASTM D638 |
| 50.0 MPa | 7250 psi | 5 mm/min; ISO 527 | |
| Tensile Strength, Yield | 65.0 MPa | 9430 psi | Type I, 50 mm/min; ASTM D638 |
| 65.0 MPa | 9430 psi | Type I, 5 mm/min; ASTM D638 | |
| Elongation at Break | 15 % | 15 % | 50 mm/min; ISO 527 |
| 100 % | 100 % | Type I, 5 mm/min; ASTM D638 | |
| Elongation at Yield | 3.5 % | 3.5 % | 5 mm/min; ISO 527 |
| 4.0 % | 4.0 % | Type I, 5 mm/min; ASTM D638 | |
| Tensile Modulus | 3.20 GPa | 464 ksi | 1 mm/min; ISO 527 |
| 3.50 GPa | 508 ksi | 5 mm/min; ASTM D638 | |
| Flexural Yield Strength | 97.0 MPa | 14100 psi | 2 mm/min; ISO 178 |
| 100 MPa | 14500 psi | 1.3 mm/min, 50 mm span; ASTM D790 | |
| Flexural Modulus | 3.30 GPa | 479 ksi | 1.3 mm/min, 50 mm span; ASTM D790 |
| 3.45 GPa | 500 ksi | 2 mm/min; ISO 178 | |
| Izod Impact, Notched | 2.00 J/cm | 3.75 ft-lb/in | ASTM D256 |
| 0.880 J/cm <br>@Temperature -30.0 °C |
1.65 ft-lb/in <br>@Temperature -22.0 °F |
ASTM D256 | |
| Izod Impact, Notched (ISO) | 10.0 kJ/m² | 4.76 ft-lb/in² | 80*10*3; ISO 180/1A |
| 5.00 kJ/m² <br>@Temperature -30.0 °C |
2.38 ft-lb/in² <br>@Temperature -22.0 °F |
80*10*3; ISO 180/1A | |
| Charpy Impact, Notched | 1.00 J/cm² | 4.76 ft-lb/in² | Edgew 80*10*3 sp=62mm; ISO 179/1eA |
| 0.500 J/cm² <br>@Temperature -30.0 °C |
2.38 ft-lb/in² <br>@Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eA | |
| Dart Drop, Total Energy | 50.0 J <br>@Temperature 23.0 °C |
36.9 ft-lb <br>@Temperature 73.4 °F |
ASTM D3763 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 55.0 µm/m-°C <br>@Temperature -40.0 - 40.0 °C |
30.6 µin/in-°F <br>@Temperature -40.0 - 104 °F |
ASTM E 831 |
| 55.0 µm/m-°C <br>@Temperature -40.0 - 40.0 °C |
30.6 µin/in-°F <br>@Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| CTE, linear, Transverse to Flow | 60.0 µm/m-°C <br>@Temperature -40.0 - 40.0 °C |
33.3 µin/in-°F <br>@Temperature -40.0 - 104 °F |
ASTM E 831 |
| 60.0 µm/m-°C <br>@Temperature -40.0 - 40.0 °C |
33.3 µin/in-°F <br>@Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| Deflection Temperature at 0.46 MPa (66 psi) | 97.0 °C <br>@Thickness 6.40 mm |
207 °F <br>@Thickness 0.252 in |
unannealed; ASTM D648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 80.0 °C | 176 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
| 83.0 °C <br>@Thickness 3.20 mm |
181 °F <br>@Thickness 0.126 in |
unannealed; ASTM D648 | |
| 89.0 °C <br>@Thickness 6.40 mm |
192 °F <br>@Thickness 0.252 in |
unannealed; ASTM D648 | |
| Vicat Softening Point | 91.0 °C | 196 °F | Rate B/50; ASTM D1525 |
| 98.0 °C | 208 °F | Rate B/50; ISO 306 | |
| 102 °C | 216 °F | Rate B/120; ISO 306 | |
| Flammability, UL94 | V-1 <br>@Thickness 0.600 mm |
V-1 <br>@Thickness 0.0236 in |
UL 94 |
| V-0 <br>@Thickness 0.800 mm |
V-0 <br>@Thickness 0.0315 in |
UL 94 | |
| 5VB <br>@Thickness 1.50 mm |
5VB <br>@Thickness 0.0591 in |
UL 94 | |
| Glow Wire Test | 800 °C | 1470 °F | IEC 60695-2-13 |
| 850 °C | 1560 °F | IEC 60695-2-13 | |
| 960 °C <br>@Thickness 0.800 mm |
1760 °F <br>@Thickness 0.0315 in |
IEC 60695-2-12 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 2.68e+16 ohm-cm | 2.68e+16 ohm-cm | ASTM D257 |
| Surface Resistance | 3.54e+15 ohm | 3.54e+15 ohm | ASTM D257 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Ball Pressure Test, 75°C +/- 2°C | PASSES95 | IEC 60695-10-2 |