| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.04 g/cc | 1.04 g/cc | ASTM D792 |
| Water Absorption | 0.19 % @Temperature 23.0 °C, Time 86400 sec |
0.19 % @Temperature 73.4 °F, Time 24.0 hour |
ASTM D570 |
| Maximum Moisture Content | 0.010 | 0.010 | Injection and Extrusion Molding |
| Linear Mold Shrinkage, Flow | 0.0040 - 0.0070 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0070 in/in @Thickness 0.126 in |
ASTM D955 |
| Melt Flow | 5.0 g/10 min @Load 10.0 kg, Temperature 220 °C |
5.0 g/10 min @Load 22.0 lb, Temperature 428 °F |
ASTM D1238 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell R | 100 | 100 | ASTM D785 |
| Tensile Strength, Yield | 42.2 MPa @Thickness 3.20 mm |
6120 psi @Thickness 0.126 in |
50 mm/min; ASTM D638 |
| Elongation at Break | >= 50 % @Thickness 3.20 mm |
>= 50 % @Thickness 0.126 in |
50 mm/min; ASTM D638 |
| Flexural Yield Strength | 60.8 MPa @Thickness 3.20 mm |
8820 psi @Thickness 0.126 in |
15 mm/min; ASTM D790 |
| Flexural Modulus | 2.16 GPa @Thickness 3.20 mm |
313 ksi @Thickness 0.126 in |
15 mm/min; ASTM D790 |
| Izod Impact, Notched | 3.14 J/cm @Thickness 6.40 mm, Temperature 23.0 °C |
5.88 ft-lb/in @Thickness 0.252 in, Temperature 73.4 °F |
ASTM D256 |
| 5.69 J/cm @Thickness 3.20 mm, Temperature 23.0 °C |
10.7 ft-lb/in @Thickness 0.126 in, Temperature 73.4 °F |
ASTM D256 | |
| Izod Impact, Unnotched | 1.47 J/cm @Thickness 6.40 mm, Temperature -20.0 °C |
2.76 ft-lb/in @Thickness 0.252 in, Temperature -4.00 °F |
ASTM D256 |
| 2.94 J/cm @Thickness 3.20 mm, Temperature -20.0 °C |
5.51 ft-lb/in @Thickness 0.126 in, Temperature -4.00 °F |
ASTM D256 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Deflection Temperature at 1.8 MPa (264 psi) | 90.0 °C @Thickness 6.40 mm |
194 °F @Thickness 0.252 in |
Unannealed; ASTM D648 |
| Vicat Softening Point | 98.0 °C @Load 5.00 kg |
208 °F @Load 11.0 lb |
50°C/h; ASTM D1525 |
| Flammability, UL94 | HB @Thickness >=0.800 mm |
HB @Thickness >=0.0315 in |
|
| HB @Thickness >=1.60 mm |
HB @Thickness >=0.0630 in |
||
| HB @Thickness >=2.50 mm |
HB @Thickness >=0.0984 in |
||
| HB @Thickness >=3.20 mm |
HB @Thickness >=0.126 in |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Rear Barrel Temperature | 180 - 200 °C | 356 - 392 °F | c |
| Middle Barrel Temperature | 190 - 210 °C | 374 - 410 °F | Injection Molding |
| Front Barrel Temperature | 200 - 220 °C | 392 - 428 °F | Injection Molding |
| Nozzle Temperature | 200 - 230 °C | 392 - 446 °F | Injection Molding |
| Zone 1 | 180 - 200 °C | 356 - 392 °F | Extrusion Molding |
| Zone 2 | 190 - 210 °C | 374 - 410 °F | Extrusion Molding |
| Zone 3 | 200 - 230 °C | 392 - 446 °F | Extrusion Molding |
| Zone 4 | 200 - 230 °C | 392 - 446 °F | Extrusion Molding |
| Adapter Temperature | 200 - 230 °C | 392 - 446 °F | Extrusion Molding |
| Die Temperature | 200 - 230 °C | 392 - 446 °F | Extrusion Molding |
| Melt Temperature | 200 - 230 °C | 392 - 446 °F | Injection and Extrusion Molding |
| Mold Temperature | 40.0 - 60.0 °C | 104 - 140 °F | Injection Molding |
| Roll Temperature | 60.0 - 90.0 °C | 140 - 194 °F | Bottom, Extrusion |
| 70.0 - 90.0 °C | 158 - 194 °F | Middle, Extrusion | |
| 70.0 - 100 °C | 158 - 212 °F | Top, Extrusion | |
| Drying Temperature | 70.0 - 80.0 °C | 158 - 176 °F | Injection and Extrusion Molding |
| Dry Time | 3.00 - 4.00 hour | 3.00 - 4.00 hour | Injection and Extrusion Molding |
| Back Pressure | 29.4 - 58.8 MPa | 4260 - 8530 psi | Injection Molding |
| Screw Speed | 30 - 60 rpm | 30 - 60 rpm | Injection Molding |