| Category | Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, 30% Glass Fiber Filled |
| Manufacturer | Eurostar Engineering Plastics |
| Trade Name | Staramide |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Eurostar Staramide BG5 PA6, 25% Glass Filled, Injection Molded.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.31 g/cc | 0.0473 lb/in³ | ISO 1183 |
| Water Absorption at Saturation | 6.5 % @Temperature 23.0 °C |
6.5 % @Temperature 73.4 °F |
ISO 62-1 |
| Linear Mold Shrinkage, Flow | 0.0020 - 0.0030 cm/cm | 0.0020 - 0.0030 in/in | on Tensile Bar; ISO 294 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 150 MPa | 21800 psi | 5 mm/min; ISO 527 |
| Elongation at Break | 3.5 % | 3.5 % | 5 mm/min; ISO 527 |
| Tensile Modulus | 7.90 GPa | 1150 ksi | 1 mm/min; ISO 527 |
| Flexural Strength | 190 MPa | 27600 psi | 2 mm/min; ISO 178 |
| Flexural Modulus | 7.80 GPa | 1130 ksi | 2 mm/min; ISO 178 |
| Izod Impact, Notched (ISO) | 7.00 kJ/m² @Temperature -40.0 °C |
3.33 ft-lb/in² @Temperature -40.0 °F |
Edgew 80x10x4 sp=62; ISO 180/1A |
| 9.00 kJ/m² @Temperature -20.0 °C |
4.28 ft-lb/in² @Temperature -4.00 °F |
Edgew 80x10x4 sp=62; ISO 180/1A | |
| 10.0 kJ/m² @Temperature 23.0 °C |
4.76 ft-lb/in² @Temperature 73.4 °F |
Edgew 80x10x4 sp=62; ISO 180/1A | |
| Charpy Impact Unnotched | 5.00 J/cm² | 23.8 ft-lb/in² | Edgew 80x10x4 sp=62; ISO 179/1eU |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 31.0 µm/m-°C @Temperature 23.0 - 60.0 °C |
17.2 µin/in-°F @Temperature 73.4 - 140 °F |
ISO 11359-2 |
| CTE, linear, Transverse to Flow | 91.0 µm/m-°C @Temperature 23.0 - 60.0 °C |
50.6 µin/in-°F @Temperature 73.4 - 140 °F |
ISO 11359-2 |
| Deflection Temperature at 0.46 MPa (66 psi) | 220 °C | 428 °F | Edgew 120x10x4, sp=100 mm; ISO 75/Bf |
| Deflection Temperature at 1.8 MPa (264 psi) | 210 °C | 410 °F | Edgew 120x10x4, sp=100 mm; ISO 75/Af |
| Vicat Softening Point | 222 °C | 432 °F | B/120; ISO 306 |
| UL RTI, Electrical | 65.0 °C @Thickness 0.750 mm |
149 °F @Thickness 0.0295 in |
|
| 65.0 °C @Thickness 1.50 mm |
149 °F @Thickness 0.0591 in |
||
| 65.0 °C @Thickness 3.00 mm |
149 °F @Thickness 0.118 in |
||
| UL RTI, Mechanical with Impact | 65.0 °C @Thickness 0.750 mm |
149 °F @Thickness 0.0295 in |
|
| 65.0 °C @Thickness 1.50 mm |
149 °F @Thickness 0.0591 in |
||
| 65.0 °C @Thickness 3.00 mm |
149 °F @Thickness 0.118 in |
||
| UL RTI, Mechanical without Impact | 65.0 °C @Thickness 0.750 mm |
149 °F @Thickness 0.0295 in |
|
| 65.0 °C @Thickness 1.50 mm |
149 °F @Thickness 0.0591 in |
||
| 65.0 °C @Thickness 3.00 mm |
149 °F @Thickness 0.118 in |
||
| Flammability, UL94 | HB @Thickness 0.750 mm |
HB @Thickness 0.0295 in |
IEC 60695-11-10 |
| HB @Thickness 1.50 mm |
HB @Thickness 0.0591 in |
IEC 60695-11-10 | |
| HB @Thickness 3.00 mm |
HB @Thickness 0.118 in |
IEC 60695-11-10 | |
| Oxygen Index | 24 % | 24 % | ISO 4589 |
| Glow Wire Test | 650 °C @Thickness 2.00 mm |
1200 °F @Thickness 0.0787 in |
IEC 60695-2-12 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | >= 1.00e+16 ohm-cm | >= 1.00e+16 ohm-cm | IEC 60093 |
| Surface Resistance | >= 1.00e+16 ohm | >= 1.00e+16 ohm | ROA; IEC 60093 |
| Dielectric Constant | 3.4 @Frequency 1.00e+6 Hz |
3.4 @Frequency 1.00e+6 Hz |
IEC 60250 |
| 3.6 @Frequency 50.0 - 60.0 Hz |
3.6 @Frequency 50.0 - 60.0 Hz |
IEC 60250 | |
| Dielectric Strength | 20.0 kV/mm @Thickness 3.20 mm |
508 kV/in @Thickness 0.126 in |
in oil; IEC 60243-1 |
| Dissipation Factor | 0.0061 @Frequency 50.0 - 60.0 Hz |
0.0061 @Frequency 50.0 - 60.0 Hz |
IEC 60250 |
| 0.016 @Frequency 1.00e+6 Hz |
0.016 @Frequency 1.00e+6 Hz |
IEC 60250 | |
| Comparative Tracking Index | 375 V | 375 V | M; IEC 60112 |
| 500 V | 500 V | IEC 60112 |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Rear Barrel Temperature | 230 - 240 °C | 446 - 464 °F | Zone 1 |
| Middle Barrel Temperature | 240 - 250 °C | 464 - 482 °F | Zone 2 |
| Front Barrel Temperature | 240 - 270 °C | 464 - 518 °F | Zone 3 |
| Melt Temperature | 240 - 270 °C | 464 - 518 °F | |
| Mold Temperature | 60.0 - 80.0 °C | 140 - 176 °F | |
| Drying Temperature | 75.0 - 85.0 °C | 167 - 185 °F | |
| Dry Time | 4.00 - 6.00 hour | 4.00 - 6.00 hour | |
| Moisture Content | 0.20 % | 0.20 % |