Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Techmer ES HiFill® PA6/6 GF/M20 IM BK 20% Glass/Mineral Fiber Filled

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, Glass Reinforced, Impact Grade , Nylon 66, Glass/Mineral Filled , Nylon 66, Heat Stabilized
Manufacturer Techmer ES
Trade Name HiFill®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Techmer ES HiFill® PA6/6 GF/M20 IM BK 20% Glass/Mineral Fiber Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 20% Filler by Weight and Mineral Filler, 20% Filler by WeightAdditive: Lubricant, Impact Modifier and Heat StabilizerFeatures: Lubricated, Impact Modified and Heat StabilizedAppearance: BlackInformation provided by TP Composites, Inc.
Physical Properties Metric English Comments
Density 1.25 g/cc
0.0452 lb/in³
ASTM D792
Water Absorption 1.2 %

@Time 86400 sec
1.2 %

@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0070 cm/cm

@Thickness 3.17 mm
0.0070 in/in

@Thickness 0.125 in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Rockwell R 112
112
ASTM D785
Tensile Strength, Yield 75.8 MPa
11000 psi
ASTM D638
Elongation at Break 4.5 %
4.5 %
ASTM D638
Flexural Strength 124 MPa
18000 psi
ASTM D790
Flexural Modulus 4.14 GPa
600 ksi
ASTM D790
Izod Impact, Notched 0.747 J/cm

@Thickness 3.17 mm
1.40 ft-lb/in

@Thickness 0.125 in
ASTM D256
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 32.4 µm/m-°C
18.0 µin/in-°F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 252 °C
485 °F
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 210 °C
410 °F
Unannealed; ASTM D648
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+15 ohm-cm
1.00e+15 ohm-cm
ASTM D257
Dielectric Strength 19.3 kV/mm
490 kV/in
Method A (Short-Time); ASTM D149
Copyright © lookpolymers.com All Rights Reserved