| Category | Polymer , Thermoplastic , Polycarbonate (PC) |
| Manufacturer | SABIC Innovative Plastics (GE Plastics) |
| Trade Name | Lexan® |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | SABIC Innovative Plastics Lexan® EXL8454 PC COPOLYMER (Asia Pacific).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.20 g/cc | 1.20 g/cc | ASTM D792 |
| Water Absorption | 0.15 % <br>@Time 86400 sec |
0.15 % <br>@Time 24.0 hour |
SABIC Method |
| Linear Mold Shrinkage, Flow | 0.0040 - 0.0080 cm/cm <br>@Thickness 3.20 mm |
0.0040 - 0.0080 in/in <br>@Thickness 0.126 in |
SABIC Method |
| Melt Flow | 10 g/10 min <br>@Load 1.20 kg,<br> Temperature 300 °C |
10 g/10 min <br>@Load 2.65 lb,<br> Temperature 572 °F |
ASTM D1238 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 55.0 MPa | 7980 psi | Type I, 50 mm/min; ASTM D638 |
| Tensile Strength, Yield | 57.0 MPa | 8270 psi | Type I, 50 mm/min; ASTM D638 |
| Elongation at Break | 100 % | 100 % | Type I, 50 mm/min; ASTM D638 |
| Elongation at Yield | 6.0 % | 6.0 % | Type I, 50 mm/min; ASTM D638 |
| Tensile Modulus | 2.20 GPa | 319 ksi | 5 mm/min; ASTM D638 |
| Flexural Yield Strength | 90.0 MPa | 13100 psi | 1.3 mm/min, 50 mm span; ASTM D790 |
| Flexural Modulus | 2.10 GPa | 305 ksi | 1.3 mm/min, 50 mm span; ASTM D790 |
| Izod Impact, Notched | 8.00 J/cm | 15.0 ft-lb/in | ASTM D256 |
| 6.50 J/cm <br>@Temperature -40.0 °C |
12.2 ft-lb/in <br>@Temperature -40.0 °F |
ASTM D256 | |
| 7.00 J/cm <br>@Temperature -30.0 °C |
13.1 ft-lb/in <br>@Temperature -22.0 °F |
ASTM D256 | |
| Charpy Impact, Notched | 6.50 J/cm² | 30.9 ft-lb/in² | Edgew 80*10*4 sp=62mm; ISO 179/1eA |
| 6.70 J/cm² | 31.9 ft-lb/in² | Edgew 80*10*3 sp=62mm; ISO 179/1eA | |
| 2.70 J/cm² <br>@Temperature -30.0 °C |
12.8 ft-lb/in² <br>@Temperature -22.0 °F |
Edgew 80*10*4 sp=62mm; ISO 179/1eA | |
| 5.40 J/cm² <br>@Temperature -40.0 °C |
25.7 ft-lb/in² <br>@Temperature -40.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eA | |
| 5.80 J/cm² <br>@Temperature -30.0 °C |
27.6 ft-lb/in² <br>@Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eA | |
| Dart Drop, Total Energy | 70.0 J <br>@Temperature 23.0 °C |
51.6 ft-lb <br>@Temperature 73.4 °F |
ASTM D3763 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 60.0 µm/m-°C <br>@Temperature -40.0 - 40.0 °C |
33.3 µin/in-°F <br>@Temperature -40.0 - 104 °F |
ASTM E 831 |
| CTE, linear, Transverse to Flow | 60.0 µm/m-°C <br>@Temperature -40.0 - 40.0 °C |
33.3 µin/in-°F <br>@Temperature -40.0 - 104 °F |
ASTM E 831 |
| Deflection Temperature at 1.8 MPa (264 psi) | 123 °C <br>@Thickness 3.20 mm |
253 °F <br>@Thickness 0.126 in |
unannealed; ASTM D648 |
| Vicat Softening Point | 145 °C | 293 °F | Rate B/50; ASTM D1525 |
| Flammability, UL94 | HB <br>@Thickness 0.750 mm |
HB <br>@Thickness 0.0295 in |
UL 94 |
| Glow Wire Test | 875 °C | 1610 °F | IEC 60695-2-13 |
| 875 °C | 1610 °F | IEC 60695-2-13 | |
| 850 °C <br>@Thickness 1.00 mm |
1560 °F <br>@Thickness 0.0394 in |
IEC 60695-2-12 | |
| 960 °C <br>@Thickness 3.00 mm |
1760 °F <br>@Thickness 0.118 in |
IEC 60695-2-12 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | >= 1.00e+15 ohm-cm | >= 1.00e+15 ohm-cm | ASTM D257 |
| Surface Resistance | >= 1.00e+15 ohm | >= 1.00e+15 ohm | ASTM D257 |
| Dielectric Constant | 3.0 <br>@Frequency 1.00e+6 Hz |
3.0 <br>@Frequency 1.00e+6 Hz |
ASTM D150 |
| Dielectric Strength | 15.0 kV/mm <br>@Thickness 0.800 mm |
381 kV/in <br>@Thickness 0.0315 in |
in oil; ASTM D149 |
| Dissipation Factor | 0.0093 <br>@Frequency 1.00e+6 Hz |
0.0093 <br>@Frequency 1.00e+6 Hz |
ASTM D150 |