Availability: North AmericaForms: PelletsFiller/Reinforcement: Carbon Fiber Reinforcement, 30% Filler by WeightAdditive: Heat StabilizerFeatures: Heat StabilizedInformation provided by TP Composites, Inc.
Physical Properties Metric English Comments
Density 1.31 g/cc
0.0473 lb/in³
ASTM D792
Water Absorption 1.9 %

@Time 86400 sec
1.9 %

@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0020 cm/cm

@Thickness 3.17 mm
0.0020 in/in

@Thickness 0.125 in
ASTM D955
Mechanical Properties Metric English Comments
Tensile Strength, Yield 228 MPa
33000 psi
ASTM D638
Elongation at Break 1.5 %
1.5 %
ASTM D638
Flexural Strength 365 MPa
53000 psi
ASTM D790
Flexural Modulus 16.5 GPa
2400 ksi
ASTM D790
Izod Impact, Notched 0.801 J/cm

@Thickness 3.17 mm
1.50 ft-lb/in

@Thickness 0.125 in
ASTM D256
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 19.8 µm/m-°C
11.0 µin/in-°F
ASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 285 °C
545 °F
Unannealed; ASTM D648
Flammability, UL94 HB
HB
Electrical Properties Metric English Comments
Volume Resistivity 10 ohm-cm
10 ohm-cm
ASTM D257