| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.18 g/cc | 1.18 g/cc | ASTM D792 |
| Density | 1.18 g/cc | 0.0426 lb/in³ | ISO 1183 |
| Moisture Absorption | 0.100 % | 0.100 % | 23°C / 50% RH; ISO 62 |
| Water Absorption at Saturation | 0.20 % | 0.20 % | ISO 62 |
| Linear Mold Shrinkage, Flow | 0.0040 - 0.0060 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0060 in/in @Thickness 0.126 in |
SABIC Method |
| Melt Flow | 22 g/10 min @Load 2.16 kg, Temperature 260 °C |
22 g/10 min @Load 4.76 lb, Temperature 500 °F |
ASTM D1238 |
| Melt Index of Compound | 18 g/10 min @Load 2.16 kg, Temperature 260 °C |
18 g/10 min @Load 4.76 lb, Temperature 500 °F |
MVR [cm^3/10 min]; ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 40.0 MPa | 5800 psi | 50 mm/min; ISO 527 |
| 45.0 MPa | 6530 psi | Type I, 50 mm/min; ASTM D638 | |
| Tensile Strength, Yield | 66.0 MPa | 9570 psi | Type I, 50 mm/min; ASTM D638 |
| 68.0 MPa | 9860 psi | 50 mm/min; ISO 527 | |
| Elongation at Break | 15 % | 15 % | 50 mm/min; ISO 527 |
| 35 % | 35 % | Type I, 50 mm/min; ASTM D638 | |
| Elongation at Yield | 3.4 % | 3.4 % | Type I, 50 mm/min; ASTM D638 |
| 3.8 % | 3.8 % | 50 mm/min; ISO 527 | |
| Tensile Modulus | 2.75 GPa | 399 ksi | 1 mm/min; ISO 527 |
| 2.95 GPa | 428 ksi | 50 mm/min; ASTM D638 | |
| Flexural Yield Strength | 100 MPa | 14500 psi | 2 mm/min; ISO 178 |
| 110 MPa | 16000 psi | 1.3 mm/min, 50 mm span; ASTM D790 | |
| Flexural Modulus | 2.60 GPa | 377 ksi | 2 mm/min; ISO 178 |
| 2.85 GPa | 413 ksi | 1.3 mm/min, 50 mm span; ASTM D790 | |
| Izod Impact, Notched | 0.750 J/cm | 1.41 ft-lb/in | ASTM D256 |
| 0.500 J/cm @Temperature -30.0 °C |
0.937 ft-lb/in @Temperature -22.0 °F |
ASTM D256 | |
| Izod Impact, Notched (ISO) | 10.0 kJ/m² | 4.76 ft-lb/in² | 80*10*3; ISO 180/1A |
| 5.00 kJ/m² @Temperature -30.0 °C |
2.38 ft-lb/in² @Temperature -22.0 °F |
80*10*3; ISO 180/1A | |
| Charpy Impact, Notched | 1.00 J/cm² | 4.76 ft-lb/in² | Edgew 80*10*3 sp=62mm; ISO 179/1eA |
| 0.500 J/cm² @Temperature -30.0 °C |
2.38 ft-lb/in² @Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eA | |
| Dart Drop, Total Energy | 40.0 J @Temperature 23.0 °C |
29.5 ft-lb @Temperature 73.4 °F |
ASTM D3763 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 60.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
33.3 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 75.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
41.7 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| CTE, linear, Transverse to Flow | 60.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
33.3 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 75.0 µm/m-°C @Temperature -40.0 - 40.0 °C |
41.7 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| Thermal Conductivity | 0.200 W/m-K | 1.39 BTU-in/hr-ft²-°F | ISO 8302 |
| Deflection Temperature at 1.8 MPa (264 psi) | 77.0 °C | 171 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
| 74.0 °C @Thickness 3.20 mm |
165 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
| 84.0 °C @Thickness 6.40 mm |
183 °F @Thickness 0.252 in |
unannealed; ASTM D648 | |
| Vicat Softening Point | 90.0 °C | 194 °F | Rate B/50; ISO 306 |
| 91.0 °C | 196 °F | Rate B/50; ASTM D1525 | |
| 95.0 °C | 203 °F | Rate B/120; ISO 306 | |
| UL RTI, Electrical | 60.0 °C | 140 °F | UL 746B |
| UL RTI, Mechanical with Impact | 60.0 °C | 140 °F | UL 746B |
| UL RTI, Mechanical without Impact | 60.0 °C | 140 °F | UL 746B |
| Flammability, UL94 | V-0 @Thickness 1.50 mm |
V-0 @Thickness 0.0591 in |
UL 94 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | >= 1.00e+15 ohm-cm | >= 1.00e+15 ohm-cm | IEC 60093 |
| Surface Resistance | >= 1.00e+15 ohm | >= 1.00e+15 ohm | ROA; IEC 60093 |
| Dielectric Strength | 17.0 kV/mm @Thickness 3.20 mm |
432 kV/in @Thickness 0.126 in |
in oil; IEC 60243-1 |
| 25.0 kV/mm @Thickness 1.60 mm |
635 kV/in @Thickness 0.0630 in |
in oil; IEC 60243-1 | |
| 35.0 kV/mm @Thickness 0.800 mm |
889 kV/in @Thickness 0.0315 in |
in oil; IEC 60243-1 | |
| Hot Wire Ignition, HWI | 15 - 30 sec | 15 - 30 sec | UL 746A |
| High Amp Arc Ignition, HAI | >= 120 arcs | >= 120 arcs | UL 746A |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Ball Pressure Test, 75°C +/- 2°C | PASSES | IEC 60695-10-2 |