Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Phenolic, Resole, Mineral Filled

Category Polymer , Thermoset , Phenolic , Phenolic, Resole, Mineral Filled
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Phenolic, Resole, Mineral Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Phenolic, Resole, Mineral Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.39 - 1.51 g/cc
0.0502 - 0.0546 lb/in³
Average value: 1.44 g/cc Grade Count:3
Water Absorption 0.360 - 0.540 %
0.360 - 0.540 %
Average value: 0.477 % Grade Count:3
Linear Mold Shrinkage 0.00300 - 0.00640 cm/cm
0.00300 - 0.00640 in/in
Average value: 0.00490 cm/cm Grade Count:3
Mechanical Properties Metric English Comments
Hardness, Rockwell E 76.0 - 83.0
76.0 - 83.0
Average value: 79.0 Grade Count:3
Tensile Strength, Ultimate 50.0 - 58.0 MPa
7250 - 8410 psi
Average value: 55.3 MPa Grade Count:3
Elongation at Break 0.660 - 0.910 %
0.660 - 0.910 %
Average value: 0.817 % Grade Count:3
Modulus of Elasticity 7.50 - 8.90 GPa
1090 - 1290 ksi
Average value: 8.30 GPa Grade Count:3
Flexural Yield Strength 85.0 - 96.0 MPa
12300 - 13900 psi
Average value: 88.7 MPa Grade Count:3
Flexural Modulus 7.10 - 8.40 GPa
1030 - 1220 ksi
Average value: 7.73 GPa Grade Count:3
Compressive Yield Strength 184 - 200 MPa
26700 - 29000 psi
Average value: 194 MPa Grade Count:3
Izod Impact, Notched 0.156 - 0.188 J/cm
0.292 - 0.352 ft-lb/in
Average value: 0.170 J/cm Grade Count:3
Charpy Impact, Notched 0.187 - 0.196 J/cm²
0.890 - 0.933 ft-lb/in²
Average value: 0.193 J/cm² Grade Count:3
Thermal Properties Metric English Comments
CTE, linear 53.0 - 53.0 µm/m-°C

@Temperature 40.0 - 130 °C
29.4 - 29.4 µin/in-°F

@Temperature 104 - 266 °F
Average value: 53.0 µm/m-°C Grade Count:1
Maximum Service Temperature, Air 182 - 205 °C
360 - 401 °F
Average value: 194 °C Grade Count:3
Deflection Temperature at 1.8 MPa (264 psi) 173 - 190 °C
343 - 374 °F
Average value: 180 °C Grade Count:3
Electrical Properties Metric English Comments
Electrical Resistivity 8.00e+12 - 4.20e+13 ohm-cm
8.00e+12 - 4.20e+13 ohm-cm
Average value: 2.47e+13 ohm-cm Grade Count:3
Dielectric Constant 5.10 - 5.80
5.10 - 5.80
Average value: 5.53 Grade Count:3
Dielectric Strength 7.50 - 13.6 kV/mm
191 - 345 kV/in
Average value: 10.7 kV/mm Grade Count:3
Dissipation Factor 0.0330 - 0.0530
0.0330 - 0.0530
Average value: 0.0427 Grade Count:3
Arc Resistance 86.0 - 141 sec
86.0 - 141 sec
Average value: 119 sec Grade Count:3
Comparative Tracking Index 175 V
175 V
Average value: 175 V Grade Count:3
Copyright © lookpolymers.com All Rights Reserved