Material Notes:
Zytel® 103FHSA NC010 is a heat stabilized, lubricated polyamide 66 for injection molding.Information provided by DuPont Performance Polymers
Physical Properties Metric English Comments
Density 1.14 g/cc
0.0412 lb/in³
DAM; ISO 1183
Water Absorption 2.8 %

@Temperature 23.0 °C
2.8 %

@Temperature 73.4 °F
Saturation, immersed; DAM; ISO 62, Similar to
8.5 %

@Temperature 23.0 °C
8.5 %

@Temperature 73.4 °F
Equilibrium 50%RH; DAM; ISO 62, Similar to
Mechanical Properties Metric English Comments
Tensile Strength, Yield 55.0 MPa

@Temperature 23.0 °C
7980 psi

@Temperature 73.4 °F
50%RH; ISO 527
85.0 MPa

@Temperature 23.0 °C
12300 psi

@Temperature 73.4 °F
DAM; ISO 527
Elongation at Break 16 %

@Temperature 23.0 °C
16 %

@Temperature 73.4 °F
DAM; nominal; ISO 527
24 %

@Temperature 23.0 °C
24 %

@Temperature 73.4 °F
DAM; ISO 527
>= 50 %

@Temperature 23.0 °C
>= 50 %

@Temperature 73.4 °F
50%RH; nominal; ISO 527
>= 50 %

@Temperature 23.0 °C
>= 50 %

@Temperature 73.4 °F
50%RH; ISO 527
Elongation at Yield 4.5 %

@Temperature 23.0 °C
4.5 %

@Temperature 73.4 °F
DAM; ISO 527
23 %

@Temperature 23.0 °C
23 %

@Temperature 73.4 °F
50%RH; ISO 527
Tensile Modulus 3.10 GPa

@Temperature 23.0 °C
450 ksi

@Temperature 73.4 °F
DAM; ISO 527
Charpy Impact Unnotched NB

@Temperature 23.0 °C
NB

@Temperature 73.4 °F
50%RH; ISO 179/1eU
NB

@Temperature 23.0 °C
NB

@Temperature 73.4 °F
DAM; ISO 179/1eU
Charpy Impact, Notched 0.500 J/cm²

@Temperature 23.0 °C
2.38 ft-lb/in²

@Temperature 73.4 °F
DAM; ISO 179/1eA
0.700 J/cm²

@Temperature 23.0 °C
3.33 ft-lb/in²

@Temperature 73.4 °F
50%RH; ISO 179/1eA
Thermal Properties Metric English Comments
Melting Point 263 °C
505 °F
10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 200 °C
392 °F
DAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °C
158 °F
DAM; ISO 75-1/-2
Processing Properties Metric English Comments
Melt Temperature 290 °C
554 °F
DAM; Optimum
280 - 300 °C
536 - 572 °F
DAM
Drying Temperature 80.0 °C
176 °F
DAM
Dry Time 2.00 - 4.00 hour
2.00 - 4.00 hour
DAM
Moisture Content <= 0.20 %
<= 0.20 %
DAM
Descriptive Properties Value Comments
Forms Pellets
DAM
Generic PA66
DAM
Material Status Preliminary Data
DAM
Processing Method Injection Molding
DAM
Product Category Unreinforced Resins
DAM
RoHS Compliance Contact Manufacturer
DAM