Physical Properties | Metric | English | Comments |
---|---|---|---|
Specific Gravity | 1.24 g/cc | 1.24 g/cc | ASTM D792 |
Density | 1.24 g/cc | 0.0448 lb/in³ | ISO 1183 |
Moisture Absorption | 0.0500 % | 0.0500 % | 23°C / 50% RH; ISO 62 |
Water Absorption at Saturation | 0.12 % | 0.12 % | ISO 62 |
Linear Mold Shrinkage, Flow | 0.0040 - 0.0080 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0080 in/in @Thickness 0.126 in |
SABIC Method |
Linear Mold Shrinkage, Transverse | 0.0040 - 0.0080 cm/cm @Thickness 3.20 mm |
0.0040 - 0.0080 in/in @Thickness 0.126 in |
SABIC Method |
Melt Flow | 8.0 g/10 min @Load 1.20 kg, Temperature 300 °C |
8.0 g/10 min @Load 2.65 lb, Temperature 572 °F |
ASTM D1238 |
Melt Index of Compound | 7.0 g/10 min @Load 1.20 kg, Temperature 300 °C |
7.0 g/10 min @Load 2.65 lb, Temperature 572 °F |
MVR [cm^3/10 min]; ISO 1133 |
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Tensile Strength at Break | 58.0 MPa | 8410 psi | 50 mm/min; ISO 527 |
58.0 MPa | 8410 psi | Type I, 50 mm/min; ASTM D638 | |
Tensile Strength, Yield | 59.0 MPa | 8560 psi | 50 mm/min; ISO 527 |
59.0 MPa | 8560 psi | Type I, 50 mm/min; ASTM D638 | |
Elongation at Break | 100 % | 100 % | 50 mm/min; ISO 527 |
100 % | 100 % | Type I, 50 mm/min; ASTM D638 | |
Elongation at Yield | 6.0 % | 6.0 % | 50 mm/min; ISO 527 |
6.0 % | 6.0 % | Type I, 50 mm/min; ASTM D638 | |
Tensile Modulus | 2.15 GPa | 312 ksi | 1 mm/min; ISO 527 |
2.15 GPa | 312 ksi | 50 mm/min; ASTM D638 | |
Flexural Yield Strength | 86.0 MPa | 12500 psi | 2 mm/min; ISO 178 |
86.0 MPa | 12500 psi | 1.3 mm/min, 50 mm span; ASTM D790 | |
Flexural Modulus | 2.15 GPa | 312 ksi | 2 mm/min; ISO 178 |
2.15 GPa | 312 ksi | 1.3 mm/min, 50 mm span; ASTM D790 | |
Izod Impact, Notched | 7.00 J/cm | 13.1 ft-lb/in | ASTM D256 |
4.50 J/cm @Temperature -50.0 °C |
8.43 ft-lb/in @Temperature -58.0 °F |
ASTM D256 | |
5.50 J/cm @Temperature -30.0 °C |
10.3 ft-lb/in @Temperature -22.0 °F |
ASTM D256 | |
Izod Impact, Notched (ISO) | 75.0 kJ/m² | 35.7 ft-lb/in² | 80*10*3; ISO 180/1A |
50.0 kJ/m² @Temperature -30.0 °C |
23.8 ft-lb/in² @Temperature -22.0 °F |
80*10*3; ISO 180/1A | |
Izod Impact, Unnotched (ISO) | NB | NB | 80*10*3; ISO 180/1U |
NB @Temperature -30.0 °C |
NB @Temperature -22.0 °F |
80*10*3; ISO 180/1U | |
Charpy Impact Unnotched | NB | NB | Edgew 80*10*3 sp=62mm; ISO 179/1eU |
NB @Temperature -30.0 °C |
NB @Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eU | |
Charpy Impact, Notched | 7.00 J/cm² | 33.3 ft-lb/in² | Edgew 80*10*3 sp=62mm; ISO 179/1eA |
5.00 J/cm² @Temperature -30.0 °C |
23.8 ft-lb/in² @Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eA |
Thermal Properties | Metric | English | Comments |
---|---|---|---|
Deflection Temperature at 0.46 MPa (66 psi) | 139 °C | 282 °F | Edgew 120*10*4 sp=100mm; ISO 75/Be |
139 °C @Thickness 3.20 mm |
282 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
Deflection Temperature at 1.8 MPa (264 psi) | 126 °C | 259 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
126 °C @Thickness 3.20 mm |
259 °F @Thickness 0.126 in |
unannealed; ASTM D648 | |
Vicat Softening Point | 145 °C | 293 °F | Rate B/50; ISO 306 |
147 °C | 297 °F | Rate B/120; ISO 306 | |
147 °C | 297 °F | Rate B/50; ASTM D1525 | |
UL RTI, Electrical | 125 °C | 257 °F | UL 746B |
UL RTI, Mechanical with Impact | 110 °C | 230 °F | UL 746B |
UL RTI, Mechanical without Impact | 125 °C | 257 °F | UL 746B |
Flammability, UL94 | V-0 @Thickness 0.800 mm |
V-0 @Thickness 0.0315 in |
UL 94 |
5VB @Thickness 2.00 mm |
5VB @Thickness 0.0787 in |
UL 94 | |
5VA @Thickness 2.50 mm |
5VA @Thickness 0.0984 in |
UL 94 | |
Glow Wire Test | 900 °C | 1650 °F | IEC 60695-2-13 |
960 °C @Thickness 0.800 - 3.00 mm |
1760 °F @Thickness 0.0315 - 0.118 in |
IEC 60695-2-12 |
Electrical Properties | Metric | English | Comments |
---|---|---|---|
Comparative Tracking Index | 250 V | 250 V | IEC 60112 |
250 - 400 V | 250 - 400 V | UL 746A | |
Hot Wire Ignition, HWI | 30 - 60 sec | 30 - 60 sec | UL 746A |
High Amp Arc Ignition, HAI | >= 120 arcs | >= 120 arcs | UL 746A |
Descriptive Properties | Value | Comments |
---|---|---|
Ball Pressure Test, 125°C +/- 2°C | PASSES | IEC 60695-10-2 |
UV-light, water exposure/immersion | F1 | UL 746C |