Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Nylon 66, Glass Fiber Filled, Flame Retardant

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, Glass Fiber Filled, Flame Retardant
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Overview of materials for Nylon 66, Glass Fiber Filled, Flame Retardant.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, Glass Fiber Filled, Flame Retardant". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.15 - 1.82 g/cc
0.0415 - 0.0658 lb/in³
Average value: 1.46 g/cc Grade Count:172
Filler Content 10.0 - 35.0 %
10.0 - 35.0 %
Average value: 24.9 % Grade Count:17
Water Absorption 0.300 - 7.00 %
0.300 - 7.00 %
Average value: 2.15 % Grade Count:60
Moisture Absorption at Equilibrium 0.170 - 2.20 %
0.170 - 2.20 %
Average value: 1.43 % Grade Count:35
Water Absorption at Saturation 3.90 - 7.00 %
3.90 - 7.00 %
Average value: 4.91 % Grade Count:12
Additive Loading 20.0 - 35.0 %
20.0 - 35.0 %
Average value: 26.6 % Grade Count:8
Viscosity Test 127 - 150 cm³/g
127 - 150 cm³/g
Average value: 141 cm³/g Grade Count:9
Linear Mold Shrinkage 0.00100 - 0.0200 cm/cm
0.00100 - 0.0200 in/in
Average value: 0.00494 cm/cm Grade Count:152
Linear Mold Shrinkage, Transverse 0.00530 - 0.105 cm/cm
0.00530 - 0.105 in/in
Average value: 0.00969 cm/cm Grade Count:54
Melt Flow 1.00 - 53.6 g/10 min
1.00 - 53.6 g/10 min
Average value: 13.8 g/10 min Grade Count:20
Mechanical Properties Metric English Comments
Hardness, Rockwell M 55.0 - 100
55.0 - 100
Average value: 87.2 Grade Count:10
Hardness, Rockwell R 101 - 122
101 - 122
Average value: 118 Grade Count:32
Hardness, Shore D 82.0 - 90.0
82.0 - 90.0
Average value: 87.0 Grade Count:3
Tensile Strength, Ultimate 50.0 - 200 MPa
7250 - 29000 psi
Average value: 132 MPa Grade Count:127
30.0 - 145 MPa
<br>@Temperature 60.0 - 150 °C
4350 - 21000 psi
<br>@Temperature 140 - 302 °F
Average value: 78.6 MPa Grade Count:14
Tensile Strength, Yield 58.0 - 180 MPa
8410 - 26100 psi
Average value: 125 MPa Grade Count:49
Elongation at Break 1.00 - 13.2 %
1.00 - 13.2 %
Average value: 2.85 % Grade Count:143
2.40 - 20.0 %
<br>@Temperature 60.0 - 150 °C
2.40 - 20.0 %
<br>@Temperature 140 - 302 °F
Average value: 4.89 % Grade Count:14
Elongation at Yield 1.40 - 7.80 %
1.40 - 7.80 %
Average value: 3.14 % Grade Count:14
3.00 - 10.0 %
<br>@Temperature 60.0 - 150 °C
3.00 - 10.0 %
<br>@Temperature 140 - 302 °F
Average value: 4.84 % Grade Count:6
Modulus of Elasticity 3.90 - 17.0 GPa
566 - 2470 ksi
Average value: 9.07 GPa Grade Count:100
0.220 - 11.5 GPa
<br>@Temperature 60.0 - 150 °C
31.9 - 1670 ksi
<br>@Temperature 140 - 302 °F
Average value: 5.24 GPa Grade Count:14
Flexural Yield Strength 90.0 - 283 MPa
13100 - 41000 psi
Average value: 190 MPa Grade Count:133
Flexural Modulus 3.70 - 12.4 GPa
537 - 1800 ksi
Average value: 7.80 GPa Grade Count:122
Compressive Yield Strength 103 - 128 MPa
15000 - 18500 psi
Average value: 117 MPa Grade Count:3
Izod Impact, Notched 0.270 - 1.33 J/cm
0.506 - 2.50 ft-lb/in
Average value: 0.776 J/cm Grade Count:80
0.69407 - 0.69407 J/cm
<br>@Temperature -40.0 - -40.0 °C
1.3003 - 1.3003 ft-lb/in
<br>@Temperature -40.0 - -40.0 °F
Average value: 0.694 J/cm Grade Count:1
Izod Impact, Unnotched 3.20 - 9.61 J/cm
6.00 - 18.0 ft-lb/in
Average value: 6.80 J/cm Grade Count:26
Izod Impact, Notched (ISO) 3.00 - 20.0 kJ/m²
1.43 - 9.52 ft-lb/in²
Average value: 8.40 kJ/m² Grade Count:37
2.00 - 11.0 kJ/m²
<br>@Temperature -40.0 - -20.0 °C
0.952 - 5.23 ft-lb/in²
<br>@Temperature -40.0 - -4.00 °F
Average value: 6.00 kJ/m² Grade Count:17
Izod Impact, Unnotched (ISO) 30.0 - 60.0 kJ/m²
14.3 - 28.6 ft-lb/in²
Average value: 47.2 kJ/m² Grade Count:10
39.0 - 47.0 kJ/m²
<br>@Temperature -30.0 - -30.0 °C
18.6 - 22.4 ft-lb/in²
<br>@Temperature -22.0 - -22.0 °F
Average value: 42.7 kJ/m² Grade Count:5
Charpy Impact Unnotched 2.00 J/cm² - NB
9.52 ft-lb/in² - NB
Average value: 5.63 J/cm² Grade Count:66
2.00 - 8.00 J/cm²
<br>@Temperature -30.0 - -20.0 °C
9.52 - 38.1 ft-lb/in²
<br>@Temperature -22.0 - -4.00 °F
Average value: 5.21 J/cm² Grade Count:26
Charpy Impact, Notched 0.200 - 1.80 J/cm²
0.952 - 8.57 ft-lb/in²
Average value: 0.953 J/cm² Grade Count:60
0.200 - 10.0 J/cm²
<br>@Temperature -30.0 - -20.0 °C
0.952 - 47.6 ft-lb/in²
<br>@Temperature -22.0 - -4.00 °F
Average value: 1.17 J/cm² Grade Count:23
Taber Abrasion, mg/1000 Cycles 24.0 - 29.0
24.0 - 29.0
Average value: 25.7 Grade Count:3
Thermal Properties Metric English Comments
CTE, linear 15.0 - 71.0 µm/m-°C
8.33 - 39.4 µin/in-°F
Average value: 35.3 µm/m-°C Grade Count:29
CTE, linear, Transverse to Flow 39.0 - 92.0 µm/m-°C
21.7 - 51.1 µin/in-°F
Average value: 75.0 µm/m-°C Grade Count:10
Specific Heat Capacity 1.40 - 1.50 J/g-°C
0.335 - 0.359 BTU/lb-°F
Average value: 1.45 J/g-°C Grade Count:4
Thermal Conductivity 0.317 - 2.20 W/m-K
2.20 - 15.3 BTU-in/hr-ft²-°F
Average value: 0.745 W/m-K Grade Count:9
Melting Point 255 - 263 °C
491 - 505 °F
Average value: 259 °C Grade Count:65
Maximum Service Temperature, Air 90.0 - 240 °C
194 - 464 °F
Average value: 154 °C Grade Count:36
Hot Ball Pressure Test 123 - 127 °C
253 - 261 °F
Average value: 125 °C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 177 - 265 °C
350 - 509 °F
Average value: 250 °C Grade Count:90
Deflection Temperature at 1.8 MPa (264 psi) 78.0 - 255 °C
172 - 491 °F
Average value: 228 °C Grade Count:137
Vicat Softening Point 215 - 258 °C
419 - 496 °F
Average value: 247 °C Grade Count:48
UL RTI, Electrical 65.0 °C
149 °F
Average value: 65.0 °C Grade Count:3
UL RTI, Mechanical with Impact 65.0 °C
149 °F
Average value: 65.0 °C Grade Count:3
Electrical Properties Metric English Comments
Electrical Resistivity 1000 - 1.00e+18 ohm-cm
1000 - 1.00e+18 ohm-cm
Average value: 3.64e+16 ohm-cm Grade Count:71
Surface Resistance 2500 - 4.00e+14 ohm
2500 - 4.00e+14 ohm
Average value: 2.37e+13 ohm Grade Count:46
Dielectric Constant 3.00 - 8.70
3.00 - 8.70
Average value: 3.91 Grade Count:37
Dielectric Strength 14.0 - 111 kV/mm
356 - 2820 kV/in
Average value: 50.0 kV/mm Grade Count:55
Dissipation Factor 0.00800 - 0.200
0.00800 - 0.200
Average value: 0.0372 Grade Count:18
Arc Resistance 130 sec
130 sec
Average value: 130 sec Grade Count:3
Comparative Tracking Index 225 - 600 V
225 - 600 V
Average value: 479 V Grade Count:68
Copyright © lookpolymers.com All Rights Reserved