Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Solvay TECHNYL® eXten D 437P PA6.10

Category Polymer , Thermoplastic , Nylon , Nylon 610
Manufacturer Solvay
Trade Name Technyl®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Solvay TECHNYL® eXten D 437P PA6.10.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Description: TECHNYL® eXten D 437P is a high viscosity, unfilled, plasticized, UV and heat stabilized PA6.10 for extrusion applications. Technyl® eXten D 437P is a partially biosourced material. This material is available in natural.Benefits: This polyamide 6,10 for extrusion is specially performing where high flexibility and toughness are requested. It is specially developed for automotive and other applications where a long term high temperature usage is requested.Key Properties: Translucency; UV stabilized; High impact at low temperature and High flexibilityAvailable in: Asia Pacific, Europe, Latin America and North America Regulations compliance: Grades produced or imported in Europe comply with directive 453/2010/EC, which amends REACH directive 1907/2006/EC This grade complies with RoHS directive 2002/95/EC Unless specified, this grade is not suitable for food contact, medical devices or toy applications Applications: Extrusion pipes and tubing applications.Information provided by Rhodia, Rhodia has been acquired by Solvay.
Physical Properties Metric English Comments
Density 1.05 g/cc
0.0379 lb/in³
ISO 1183/A
Viscosity 700 cP

@Shear Rate 1000 1/s,
Temperature 230 °C
700 cP

@Shear Rate 1000 1/s,
Temperature 446 °F
1000 cP

@Shear Rate 100 1/s,
Temperature 230 °C
1000 cP

@Shear Rate 100 1/s,
Temperature 446 °F
5000 cP

@Shear Rate 10.0 1/s,
Temperature 230 °C
5000 cP

@Shear Rate 10.0 1/s,
Temperature 446 °F
Linear Mold Shrinkage 0.0104 cm/cm
0.0104 in/in
Isotropy
Linear Mold Shrinkage, Flow 0.0242 cm/cm
0.0242 in/in
Linear Mold Shrinkage, Transverse 0.0233 cm/cm
0.0233 in/in
Mechanical Properties Metric English Comments
Tensile Strength at Break 50.0 MPa
7250 psi
ISO 527 Type 1A
Tensile Stress 12.0 MPa

@Strain 20.0 %,
Temperature 150 °C
1740 psi

@Strain 20.0 %,
Temperature 302 °F
12.0 MPa

@Strain 100 %,
Temperature 150 °C
1740 psi

@Strain 100 %,
Temperature 302 °F
15.0 MPa

@Strain 20.0 %,
Temperature 135 °C
2180 psi

@Strain 20.0 %,
Temperature 275 °F
15.0 MPa

@Strain 160 %,
Temperature 150 °C
2180 psi

@Strain 160 %,
Temperature 302 °F
16.0 MPa

@Strain 100 %,
Temperature 135 °C
2320 psi

@Strain 100 %,
Temperature 275 °F
20.0 MPa

@Strain 160 %,
Temperature 135 °C
2900 psi

@Strain 160 %,
Temperature 275 °F
23.0 MPa

@Strain 20.0 %,
Temperature 80.0 °C
3340 psi

@Strain 20.0 %,
Temperature 176 °F
27.0 MPa

@Strain 100 %,
Temperature 80.0 °C
3920 psi

@Strain 100 %,
Temperature 176 °F
30.0 MPa

@Strain 160 %,
Temperature 80.0 °C
4350 psi

@Strain 160 %,
Temperature 176 °F
40.0 MPa

@Strain 20.0 %,
Temperature 23.0 °C
5800 psi

@Strain 20.0 %,
Temperature 73.4 °F
41.0 MPa

@Strain 100 %,
Temperature 23.0 °C
5950 psi

@Strain 100 %,
Temperature 73.4 °F
43.0 MPa

@Strain 160 %,
Temperature 23.0 °C
6240 psi

@Strain 160 %,
Temperature 73.4 °F
Elongation at Break 215 %
215 %
ISO 527 Type 1A
Tensile Modulus 0.890 GPa
129 ksi
ISO 527 Type 1A
Flexural Strength 33.0 MPa
4790 psi
ISO 178
Flexural Modulus 0.720 GPa
104 ksi
ISO 178
Charpy Impact Unnotched NB

@Temperature 23.0 °C
NB

@Temperature 73.4 °F
ISO 179/1eU
NB

@Temperature -30.0 °C
NB

@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.400 J/cm²

@Temperature -30.0 °C
1.90 ft-lb/in²

@Temperature -22.0 °F
ISO 179/1eA
2.50 J/cm²

@Temperature 23.0 °C
11.9 ft-lb/in²

@Temperature 73.4 °F
ISO 179/1eA
Thermal Properties Metric English Comments
Melting Point 215 °C
419 °F
ISO 11357
Flammability, UL94 HB

@Thickness 0.800 mm
HB

@Thickness 0.0315 in
ISO 1210
HB

@Thickness 1.60 mm
HB

@Thickness 0.0630 in
ISO 1210
HB

@Thickness 3.20 mm
HB

@Thickness 0.126 in
ISO 1210
Processing Properties Metric English Comments
Feed Temperature 200 - 220 °C
392 - 428 °F
Drying Temperature 80.0 °C

@Time 28800 sec
176 °F

@Time 8.00 hour
dew point -35°C
Moisture Content <= 0.10 %
<= 0.10 %
Descriptive Properties Value Comments
Compression Zone 210-230°C