This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, 50% Glass Fiber Filled". Specific grades with glass content between 45% and 54% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.45 - 1.78 g/cc
0.0524 - 0.0643 lb/in³
Average value: 1.57 g/cc Grade Count:144
1.40 - 1.40 g/cc

@Temperature 295 - 295 °C
0.0506 - 0.0506 lb/in³

@Temperature 563 - 563 °F
Average value: 1.40 g/cc Grade Count:1
Filler Content 45.0 - 50.0 %
45.0 - 50.0 %
Average value: 49.4 % Grade Count:27
Water Absorption 0.300 - 4.30 %
0.300 - 4.30 %
Average value: 1.77 % Grade Count:71
1.10 - 1.50 %

@Temperature 70.0 - 70.0 °C
1.10 - 1.50 %

@Temperature 158 - 158 °F
Average value: 1.25 % Grade Count:4
Moisture Absorption at Equilibrium 0.170 - 2.00 %
0.170 - 2.00 %
Average value: 1.15 % Grade Count:43
Water Absorption at Saturation 0.200 - 7.00 %
0.200 - 7.00 %
Average value: 3.64 % Grade Count:21
Viscosity 8000 - 160000 cP

@Temperature 277 - 322 °C
8000 - 160000 cP

@Temperature 531 - 612 °F
Average value: 47200 cP Grade Count:1
8000 - 160000 cP

@Frequency 10.0 - 10000 Hz
8000 - 160000 cP

@Frequency 10.0 - 10000 Hz
Average value: 47200 cP Grade Count:1
20.0 - 450 cP

@Temperature 280 - 300 °C
20.0 - 450 cP

@Temperature 536 - 572 °F
Average value: 47200 cP Grade Count:1
20.0 - 450 cP

@Shear Rate 10.0 - 1000 1/s
20.0 - 450 cP

@Shear Rate 10.0 - 1000 1/s
Average value: 47200 cP Grade Count:1
Viscosity Test 131 - 150 cm³/g
131 - 150 cm³/g
Average value: 139 cm³/g Grade Count:8
Maximum Moisture Content 0.0900 - 0.900
0.0900 - 0.900
Average value: 0.360 Grade Count:3
Linear Mold Shrinkage 0.00100 - 0.0200 cm/cm
0.00100 - 0.0200 in/in
Average value: 0.00332 cm/cm Grade Count:117
Linear Mold Shrinkage, Transverse 0.00150 - 0.0120 cm/cm
0.00150 - 0.0120 in/in
Average value: 0.00781 cm/cm Grade Count:53
Melt Flow 1.00 - 40.0 g/10 min
1.00 - 40.0 g/10 min
Average value: 18.4 g/10 min Grade Count:19
Spiral Flow 54.0 - 536 cm
21.3 - 211 in
Average value: 138 cm Grade Count:6
Mechanical Properties Metric English Comments
Hardness, Rockwell M 80.0 - 97.0
80.0 - 97.0
Average value: 90.5 Grade Count:3
Hardness, Rockwell R 98.0 - 125
98.0 - 125
Average value: 120 Grade Count:34
Ball Indentation Hardness 131 - 340 MPa
19000 - 49300 psi
Average value: 303 MPa Grade Count:15
Tensile Strength, Ultimate 30.0 - 299 MPa
4350 - 43400 psi
Average value: 219 MPa Grade Count:91
65.0 - 342.669 MPa

@Temperature -40.0 - 150 °C
9430 - 49700.1 psi

@Temperature -40.0 - 302 °F
Average value: 128 MPa Grade Count:9
110 - 125 MPa

@Temperature 130 - 175 °C
16000 - 18100 psi

@Temperature 266 - 347 °F
Average value: 128 MPa Grade Count:4
110 - 125 MPa

@Time 1.80e+7 - 7.20e+7 sec
16000 - 18100 psi

@Time 5000 - 20000 hour
Average value: 128 MPa Grade Count:4
25.0 - 195 MPa

@Strain 0.500 - 8.00 %
3630 - 28300 psi

@Strain 0.500 - 8.00 %
Average value: 128 MPa Grade Count:1
25.0 - 195 MPa

@Temperature 60.0 - 120 °C
3630 - 28300 psi

@Temperature 140 - 248 °F
Average value: 128 MPa Grade Count:1
Tensile Strength, Yield 130 - 265 MPa
18900 - 38400 psi
Average value: 212 MPa Grade Count:54
131 - 265 MPa

@Temperature -20.0 - 93.3 °C
19000 - 38400 psi

@Temperature -4.00 - 200 °F
Average value: 179 MPa Grade Count:2
Elongation at Break 1.00 - 5.00 %
1.00 - 5.00 %
Average value: 2.48 % Grade Count:123
1.80 - 8.00 %

@Temperature 4.44 - 150 °C
1.80 - 8.00 %

@Temperature 40.0 - 302 °F
Average value: 4.18 % Grade Count:8
Elongation at Yield 1.00 - 3.70 %
1.00 - 3.70 %
Average value: 2.63 % Grade Count:13
Modulus of Elasticity 10.2 - 18.7 GPa
1480 - 2710 ksi
Average value: 15.5 GPa Grade Count:101
4.00 - 19.788 GPa

@Temperature -40.0 - 200 °C
580 - 2870.0 ksi

@Temperature -40.0 - 392 °F
Average value: 8.59 GPa Grade Count:9
Flexural Yield Strength 216 - 425 MPa
31300 - 61600 psi
Average value: 326 MPa Grade Count:106
175 - 455.054 MPa

@Temperature -40.0 - 149 °C
25400 - 66000.1 psi

@Temperature -40.0 - 300 °F
Average value: 264 MPa Grade Count:6
Flexural Modulus 7.90 - 17.2 GPa
1150 - 2500 ksi
Average value: 13.9 GPa Grade Count:111
6.60 - 19.0985 GPa

@Temperature -40.0 - 149 °C
957 - 2770.04 ksi

@Temperature -40.0 - 300 °F
Average value: 10.3 GPa Grade Count:7
Izod Impact, Notched 1.01 - 6.51 J/cm
1.90 - 12.2 ft-lb/in
Average value: 1.97 J/cm Grade Count:57
1.10 - 7.36782 J/cm

@Temperature -40.0 - 149 °C
2.06 - 13.8029 ft-lb/in

@Temperature -40.0 - 300 °F
Average value: 3.97 J/cm Grade Count:2
Izod Impact, Unnotched 9.61 - 70.0 J/cm
18.0 - 131 ft-lb/in
Average value: 15.2 J/cm Grade Count:24
Izod Impact, Notched (ISO) 12.0 - 54.0 kJ/m²
5.71 - 25.7 ft-lb/in²
Average value: 17.4 kJ/m² Grade Count:29
11.0 - 47.0 kJ/m²

@Temperature -40.0 - -20.0 °C
5.23 - 22.4 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 16.1 kJ/m² Grade Count:13
Izod Impact, Unnotched (ISO) 80.0 - 103 kJ/m²
38.1 - 49.0 ft-lb/in²
Average value: 90.6 kJ/m² Grade Count:5
90.0 - 96.0 kJ/m²

@Temperature -30.0 - -30.0 °C
42.8 - 45.7 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 92.0 kJ/m² Grade Count:3
Charpy Impact Unnotched 4.50 J/cm² - NB
21.4 ft-lb/in² - NB
Average value: 9.06 J/cm² Grade Count:71
4.60 J/cm² - NB

@Temperature -40.0 - 30.0 °C
21.9 ft-lb/in² - NB

@Temperature -40.0 - 86.0 °F
Average value: 8.46 J/cm² Grade Count:40
Charpy Impact, Notched 0.500 - 4.70 J/cm²
2.38 - 22.4 ft-lb/in²
Average value: 1.83 J/cm² Grade Count:72
0.350 - 4.50 J/cm²

@Temperature -40.0 - 30.0 °C
1.67 - 21.4 ft-lb/in²

@Temperature -40.0 - 86.0 °F
Average value: 1.39 J/cm² Grade Count:39
Dart Drop, Total Energy 9.99 - 23.5 J

@Temperature -20.0 - -20.0 °C
7.37 - 17.3 ft-lb

@Temperature -4.00 - -4.00 °F
Average value: 16.7 J Grade Count:1
9.99 - 23.5 J

@Thickness 3.18 - 3.18 mm
7.37 - 17.3 ft-lb

@Thickness 0.125 - 0.125 in
Average value: 16.7 J Grade Count:1
Puncture Energy 2.80 - 2.80 J

@Temperature -30.0 - -30.0 °C
2.07 - 2.07 ft-lb

@Temperature -22.0 - -22.0 °F
Average value: 2.80 J Grade Count:1