| Category | Polymer , Thermoplastic , Nylon , Nylon 612 , Nylon 612, Glass Fiber Filler |
| Manufacturer | DuPont Performance Polymers |
| Trade Name | Zytel® |
| Port | Ningbo port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | DuPont Performance Polymers Zytel® 77G33HS1L NC010 Nylon 612.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.32 g/cc | 1.32 g/cc | DAM; ASTM D792 |
| Density | 1.32 g/cc | 0.0477 lb/in³ | DAM; ISO 1183 |
| Filler Content | 33 % | 33 % | DAM |
| Water Absorption | 0.16 % @Temperature 23.0 °C |
0.16 % @Temperature 73.4 °F |
Immersion 24h; DAM; ASTM D570 |
| 2.0 % @Temperature 23.0 °C |
2.0 % @Temperature 73.4 °F |
Saturation; DAM; ASTM D570 | |
| 0.70 % @Thickness 1.00 mm, Temperature 23.0 °C |
0.70 % @Thickness 0.0394 in, Temperature 73.4 °F |
Equilibrium 50%RH; DAM; ISO 62, Similar to | |
| 1.8 % @Thickness 1.00 mm, Temperature 23.0 °C |
1.8 % @Thickness 0.0394 in, Temperature 73.4 °F |
Saturation, immersed; DAM; ISO 62, Similar to | |
| Linear Mold Shrinkage | 0.0010 cm/cm @Thickness 1.60 mm |
0.0010 in/in @Thickness 0.0630 in |
Flow; DAM |
| 0.0020 cm/cm @Thickness 3.20 mm |
0.0020 in/in @Thickness 0.126 in |
Flow; DAM | |
| 0.0040 cm/cm @Thickness 6.40 mm |
0.0040 in/in @Thickness 0.252 in |
Flow; DAM | |
| 0.0090 cm/cm @Thickness 1.60 mm |
0.0090 in/in @Thickness 0.0630 in |
Transverse; DAM | |
| 0.010 cm/cm @Thickness 3.20 mm |
0.010 in/in @Thickness 0.126 in |
Transverse; DAM | |
| 0.011 cm/cm @Thickness 6.40 mm |
0.011 in/in @Thickness 0.252 in |
Transverse; DAM | |
| Linear Mold Shrinkage, Flow | 0.0030 cm/cm @Thickness 2.00 mm |
0.0030 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Linear Mold Shrinkage, Transverse | 0.0090 cm/cm @Thickness 2.00 mm |
0.0090 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell R | 118 | 118 | DAM; ASTM D785 |
| Tensile Strength at Break | 140 MPa @Temperature 23.0 °C |
20300 psi @Temperature 73.4 °F |
50%RH; ISO 527 |
| 168 MPa @Temperature 23.0 °C |
24400 psi @Temperature 73.4 °F |
DAM; ISO 527 | |
| Tensile Strength | 138 MPa @Temperature 23.0 °C |
20000 psi @Temperature 73.4 °F |
50%RH; ASTM D638 |
| 165 MPa @Temperature 23.0 °C |
23900 psi @Temperature 73.4 °F |
DAM; ASTM D638 | |
| Elongation at Break | 3.0 % @Temperature 23.0 °C |
3.0 % @Temperature 73.4 °F |
DAM; ASTM D638 |
| 3.0 % @Temperature 23.0 °C |
3.0 % @Temperature 73.4 °F |
DAM; ISO 527 | |
| 3.2 % @Temperature 23.0 °C |
3.2 % @Temperature 73.4 °F |
50%RH; ISO 527 | |
| 4.0 % @Temperature 23.0 °C |
4.0 % @Temperature 73.4 °F |
50%RH; ASTM D638 | |
| Tensile Modulus | 7.90 GPa @Temperature 23.0 °C |
1150 ksi @Temperature 73.4 °F |
50%RH; ISO 527 |
| 9.50 GPa @Temperature 23.0 °C |
1380 ksi @Temperature 73.4 °F |
DAM; ISO 527 | |
| Flexural Strength | 255 MPa @Temperature 23.0 °C |
37000 psi @Temperature 73.4 °F |
DAM; ASTM D790 |
| Flexural Modulus | 6.20 GPa @Temperature 23.0 °C |
899 ksi @Temperature 73.4 °F |
50%RH; ASTM D790 |
| 7.00 GPa @Temperature 23.0 °C |
1020 ksi @Temperature 73.4 °F |
50%RH; ISO 178 | |
| 8.20 GPa @Temperature 23.0 °C |
1190 ksi @Temperature 73.4 °F |
DAM; ISO 178 | |
| 8.27 GPa @Temperature 23.0 °C |
1200 ksi @Temperature 73.4 °F |
DAM; ASTM D790 | |
| Shear Strength | 76.0 MPa @Temperature 23.0 °C |
11000 psi @Temperature 73.4 °F |
DAM; ASTM D732 |
| Izod Impact, Notched | 1.28 J/cm @Temperature 23.0 °C |
2.40 ft-lb/in @Temperature 73.4 °F |
DAM; ASTM D256 |
| 1.33 J/cm @Temperature 23.0 °C |
2.49 ft-lb/in @Temperature 73.4 °F |
50%RH; ASTM D256 | |
| Izod Impact, Notched (ISO) | 10.0 kJ/m² @Temperature -40.0 °C |
4.76 ft-lb/in² @Temperature -40.0 °F |
50%RH; ISO 180/1A |
| 10.0 kJ/m² @Temperature -30.0 °C |
4.76 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 180/1A | |
| 11.0 kJ/m² @Temperature -40.0 °C |
5.23 ft-lb/in² @Temperature -40.0 °F |
DAM; ISO 180/1A | |
| 11.0 kJ/m² @Temperature -30.0 °C |
5.23 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 180/1A | |
| 12.0 kJ/m² @Temperature 23.0 °C |
5.71 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 180/1A | |
| 13.0 kJ/m² @Temperature 23.0 °C |
6.19 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 180/1A | |
| Izod Impact, Unnotched (ISO) | 45.0 kJ/m² @Temperature -30.0 °C |
21.4 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 180/1U |
| 60.0 kJ/m² @Temperature -30.0 °C |
28.6 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 180/1U | |
| 60.0 kJ/m² @Temperature 23.0 °C |
28.6 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 180/1U | |
| 70.0 kJ/m² @Temperature 23.0 °C |
33.3 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 180/1U | |
| Charpy Impact Unnotched | 6.00 J/cm² @Temperature -30.0 °C |
28.6 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eU |
| 6.50 J/cm² @Temperature -30.0 °C |
30.9 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eU | |
| 8.00 J/cm² @Temperature 23.0 °C |
38.1 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 179/1eU | |
| 9.00 J/cm² @Temperature 23.0 °C |
42.8 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 179/1eU | |
| Charpy Impact, Notched | 1.00 J/cm² @Temperature -30.0 °C |
4.76 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eA |
| 1.00 J/cm² @Temperature -40.0 °C |
4.76 ft-lb/in² @Temperature -40.0 °F |
50%RH; ISO 179/1eA | |
| 1.10 J/cm² @Temperature -30.0 °C |
5.23 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eA | |
| 1.20 J/cm² @Temperature 23.0 °C |
5.71 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 179/1eA | |
| 1.20 J/cm² @Temperature -40.0 °C |
5.71 ft-lb/in² @Temperature -40.0 °F |
DAM; ISO 179/1eA | |
| 1.30 J/cm² @Temperature 23.0 °C |
6.19 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 179/1eA |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 500 µm/m-°C @Temperature -40.0 - 23.0 °C |
278 µin/in-°F @Temperature -40.0 - 73.4 °F |
DAM; ASTM E 831 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 1.00e+12 ohm-cm @Temperature 23.0 °C |
1.00e+12 ohm-cm @Temperature 73.4 °F |
50%RH; ASTM D257 |
| 1.00e+15 ohm-cm @Temperature 23.0 °C |
1.00e+15 ohm-cm @Temperature 73.4 °F |
DAM; ASTM D257 | |
| 1.00e+15 ohm-cm @Temperature 23.0 °C |
1.00e+15 ohm-cm @Temperature 73.4 °F |
DAM; IEC 60093 | |
| Surface Resistance | 1.00e+15 ohm @Temperature 23.0 °C |
1.00e+15 ohm @Temperature 73.4 °F |
DAM; ASTM D257 |
| Dielectric Constant | 3.4 @Frequency 1.00e+6 Hz, Temperature 23.0 °C |
3.4 @Frequency 1.00e+6 Hz, Temperature 73.4 °F |
DAM; ASTM D150 |
| 3.7 @Frequency 1000 Hz, Temperature 23.0 °C |
3.7 @Frequency 1000 Hz, Temperature 73.4 °F |
DAM; ASTM D150 | |
| Dielectric Strength | 20.5 kV/mm @Thickness 3.20 mm, Temperature 23.0 °C |
521 kV/in @Thickness 0.126 in, Temperature 73.4 °F |
DAM; Short Time; ASTM D149 |
| Dissipation Factor | 0.020 @Frequency 1000 Hz, Temperature 23.0 °C |
0.020 @Frequency 1000 Hz, Temperature 73.4 °F |
DAM; ASTM D150 |
| 0.020 @Frequency 1.00e+6 Hz, Temperature 23.0 °C |
0.020 @Frequency 1.00e+6 Hz, Temperature 73.4 °F |
DAM; ASTM D150 | |
| Comparative Tracking Index | >= 550 V @Temperature 23.0 °C |
>= 550 V @Temperature 73.4 °F |
DAM; UL 746A |
| 600 V @Temperature 23.0 °C |
600 V @Temperature 73.4 °F |
DAM; IEC 60112 |