Material Notes:
Cold Formable Medium-Strength AlloyIndustry Specifications: Germany Aerospace: 3.7124. France: T-U2. UK Aerospace Specifications BA TA. 21, 22, 23.Features: This binary, age hardening alloy combines the easy formability and weldability of commercially pure titanium with improved mechanical properties, particularly at temperatures up to 350°C. It is used in the annealed condition as sheet, forgings, and extrusions for fabricating components such as bypass ducts of gas-turbine engines. Its used spread to the airframe industry, following the development of an ageing treatment which raises room-temperature tensile properties by about 25%, and nearly doubles the elevated temperature properties. Such a material is particularly attractive since it can be formed in the soft condition, thus lowering fabrication costs. It is nonmagnetic.Typical heat treatment for this alloy: Anneal at 790°C for 1 hour and air cool. Solution heat treatment at 805°C for 1 hour with a rapid air cool. Aging heat treatment at 400°C for 8-24 hours with an air cool and then for 8 hours at 475°C with air cool.Data provided by TIMET.
Physical Properties Metric English Comments
Density 4.56 g/cc
0.165 lb/in³
Typical
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 620 MPa
89900 psi
Typical
Tensile Strength, Yield 510 MPa

@Strain 0.200 %
74000 psi

@Strain 0.200 %
Typical
Elongation at Break 25 %
25 %
Typical
Reduction of Area >= 35 %
>= 35 %
Modulus of Elasticity 105 - 120 GPa
15200 - 17400 ksi
Typical
Fatigue Strength 280 MPa

@# of Cycles 1.00e+7
40600 psi

@# of Cycles 1.00e+7
Rod, smooth, direct stress
370 MPa

@# of Cycles 1.00e+7
53700 psi

@# of Cycles 1.00e+7
Rod, rotating bend
390 MPa

@# of Cycles 1.00e+7
56600 psi

@# of Cycles 1.00e+7
Sheet; Reverse Bend; (UTS = 864 MPa)
Bend Radius, Minimum 2.5 t

@Thickness 2.00 mm
2.5 t

@Thickness 0.0787 in
Typical; sheet
Thermal Properties Metric English Comments
CTE, linear 9.00 µm/m-°C

@Temperature 20.0 - 100 °C
5.00 µin/in-°F

@Temperature 68.0 - 212 °F
Thermal Conductivity 12.97 W/m-K
90.01 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 350 °C
662 °F
Beta Transus 895 °C
1640 °F
Component Elements Properties Metric English Comments
Carbon, C <= 0.080 %
<= 0.080 %
Copper, Cu 2.0 - 3.0 %
2.0 - 3.0 %
Hydrogen, H <= 0.010 %
<= 0.010 %
Iron, Fe <= 0.20 %
<= 0.20 %
Nitrogen, N <= 0.030 %
<= 0.030 %
Oxygen, O <= 0.20 %
<= 0.20 %
Titanium, Ti 96.1 - 98 %
96.1 - 98 %
Calculated as remainder
Electrical Properties Metric English Comments
Electrical Resistivity 0.0000650 ohm-cm
0.0000650 ohm-cm
Copyright © lookpolymers.com All Rights Reserved