Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

SABIC Innovative Plastics Xylex HX7409HP PC+POLYESTER (Asia Pacific)

Category Polymer , Thermoplastic , Polycarbonate (PC) , Polycarbonate/PET Polyester Blend , Polyester, TP , Polyethylene Terephthalate (PET)
Manufacturer SABIC Innovative Plastics (GE Plastics)
Trade Name Xylex
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF SABIC Innovative Plastics Xylex HX7409HP PC+POLYESTER (Asia Pacific).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Low flow, polycarbonate/Polyester alloy; contains mold release. For medical devices and pharmaceutical applications. Healthcare management of change (MoC), biocompatible (ISO 10993 or USP Class VI), food contact compliant. EtO and gamma sterilizable.This data was supplied by SABIC-IP for the Asia Pacific region.
Physical Properties Metric English Comments
Specific Gravity 1.20 g/cc
1.20 g/cc
ASTM D 792
Density 1.20 g/cc
0.0434 lb/in³
ISO 1183
Moisture Absorption at Equilibrium 0.070 %
0.070 %
23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.28 %

@Temperature 23.0 °C
0.28 %

@Temperature 73.4 °F
ISO 62
Linear Mold Shrinkage, Flow 0.0060 - 0.0080 cm/cm

@Thickness 3.20 mm
0.0060 - 0.0080 in/in

@Thickness 0.126 in
SABIC Method
Linear Mold Shrinkage, Transverse 0.0060 - 0.0080 cm/cm

@Thickness 3.20 mm
0.0060 - 0.0080 in/in

@Thickness 0.126 in
SABIC Method
Melt Flow 3.0 g/10 min

@Load 2.16 kg,
Temperature 265 °C
3.0 g/10 min

@Load 4.76 lb,
Temperature 509 °F
ASTM D 1238
15 g/10 min

@Load 10.0 kg,
Temperature 265 °C
15 g/10 min

@Load 22.0 lb,
Temperature 509 °F
[cm^3/10 min] Melt Volume Rate; ISO 1133
Mechanical Properties Metric English Comments
Tensile Strength at Break 65.0 MPa
9430 psi
50 mm/min; ISO 527
65.0 MPa
9430 psi
Type I, 50 mm/min; ASTM D 638
Tensile Strength, Yield 60.0 MPa
8700 psi
50 mm/min; ISO 527
62.0 MPa
8990 psi
Type I, 50 mm/min; ASTM D 638
Elongation at Break 110 %
110 %
Type I, 50 mm/min; ASTM D 638
135 %
135 %
50 mm/min; ISO 527
Elongation at Yield 6.0 %
6.0 %
50 mm/min; ISO 527
6.0 %
6.0 %
Type I, 50 mm/min; ASTM D 638
Tensile Modulus 2.30 GPa
334 ksi
50 mm/min; ASTM D 638
2.40 GPa
348 ksi
1 mm/min; ISO 527
Flexural Yield Strength 93.0 MPa
13500 psi
2 mm/min; ISO 178
95.0 MPa
13800 psi
1.3 mm/min, 50 mm span; ASTM D 790
Flexural Modulus 2.18 GPa
316 ksi
2 mm/min; ISO 178
2.28 GPa
331 ksi
1.3 mm/min, 50 mm span; ASTM D 790
Izod Impact, Notched 0.800 J/cm

@Temperature -30.0 °C
1.50 ft-lb/in

@Temperature -22.0 °F
ASTM D 256
10.0 J/cm

@Temperature 23.0 °C
18.7 ft-lb/in

@Temperature 73.4 °F
ASTM D 256
Izod Impact, Notched (ISO) 6.00 kJ/m²

@Temperature -30.0 °C
2.86 ft-lb/in²

@Temperature -22.0 °F
80*10*4; ISO 180/1A
15.0 kJ/m²

@Temperature 23.0 °C
7.14 ft-lb/in²

@Temperature 73.4 °F
80*10*4; ISO 180/1A
78.0 kJ/m²

@Temperature 23.0 °C
37.1 ft-lb/in²

@Temperature 73.4 °F
63.5*12.7*3.2; ISO 180/4A
Charpy Impact, Notched 2.20 J/cm²

@Temperature 23.0 °C
10.5 ft-lb/in²

@Temperature 73.4 °F
V-notch Edgew 80*10*4 sp=62mm; ISO 179/1eA
Impact Test 85.0 J

@Temperature 23.0 °C
62.7 ft-lb

@Temperature 73.4 °F
Instrumented Impact Total Energy; ASTM D 3763
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 70.0 µm/m-°C

@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F

@Temperature -40.0 - 104 °F
ISO 11359-2
70.0 µm/m-°C

@Temperature -40.0 - 95.0 °C
38.9 µin/in-°F

@Temperature -40.0 - 203 °F
ASTM E 831
CTE, linear, Transverse to Flow 70.0 µm/m-°C

@Temperature -40.0 - 95.0 °C
38.9 µin/in-°F

@Temperature -40.0 - 203 °F
ASTM E 831
70.0 µm/m-°C

@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F

@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 122 °C
252 °F
Edgew 120*10*4 sp=100mm; ISO 75/Be
122 °C

@Thickness 3.20 mm
252 °F

@Thickness 0.126 in
unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi) 111 °C
232 °F
Edgew 120*10*4 sp=100mm; ISO 75/Ae
111 °C

@Thickness 3.20 mm
232 °F

@Thickness 0.126 in
unannealed; ASTM D 648
Vicat Softening Point 127 °C
261 °F
Rate B/50; ISO 306
129 °C
264 °F
Rate B/120; ISO 306
130 °C
266 °F
Rate B/50; ASTM D 1525
Optical Properties Metric English Comments
Transmission, Visible 79 %

@Thickness 2.54 mm
79 %

@Thickness 0.100 in
ASTM D 1003