Material Notes:
Radilon® S is a range of polyamide 6 (PA6) products obtained through the polymerization of caprolactam and used for injection, extrusion and blow-molding.Information provided by Radici group.
Physical Properties Metric English Comments
Specific Gravity 1.21 g/cc
1.21 g/cc
Water Absorption 8.8 %
8.8 %
Moisture Absorption at Equilibrium 2.4 %
2.4 %
Viscosity Measurement 145
145
cm³/g Viscosity Number
Mechanical Properties Metric English Comments
Tensile Strength at Break 125 MPa
18100 psi
Elongation at Break 3.9 %
3.9 %
Tensile Modulus 6.05 GPa
877 ksi
Charpy Impact Unnotched 4.40 J/cm²

@Temperature 23.0 °C
20.9 ft-lb/in²

@Temperature 73.4 °F
4.40 J/cm²

@Temperature -30.0 °C
20.9 ft-lb/in²

@Temperature -22.0 °F
Charpy Impact, Notched 0.570 J/cm²

@Temperature -30.0 °C
2.71 ft-lb/in²

@Temperature -22.0 °F
0.700 J/cm²

@Temperature 23.0 °C
3.33 ft-lb/in²

@Temperature 73.4 °F
Thermal Properties Metric English Comments
Melting Point 220 °C
428 °F
Deflection Temperature at 0.46 MPa (66 psi) 200 °C
392 °F
Deflection Temperature at 1.8 MPa (264 psi) 180 °C
356 °F
Vicat Softening Point 210 °C

@Load 5.10 kg
410 °F

@Load 11.2 lb
50°C/h
Flammability, UL94 HB

@Thickness 1.60 mm
HB

@Thickness 0.0630 in
HB

@Thickness 0.800 mm
HB

@Thickness 0.0315 in
Electrical Properties Metric English Comments
Volume Resistivity >= 1.00e+11 ohm-cm
>= 1.00e+11 ohm-cm