Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

NatureWorks® Ingeo™ AW 300D Injection Grade Biopolymer

Category Polymer , Renewable/Recycled Polymer , Thermoplastic , Polylactic Acid (PLA) Biopolymer
Manufacturer NatureWorks LLC
Trade Name Ingeo™
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF NatureWorks® Ingeo™ AW 300D Injection Grade Biopolymer.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Specifically designed for use in injection molded food serviceware applications. This opaque, off-white molding grade creates parts that are rigid and heat resistant for tableware used with hot foods and drinks when injection molded using conventional chilled molds. Ingeo AW 300D is fully formulated to be used naturally, but may be blended with color compounds.Information provided by NatureWorks LLC.
Physical Properties Metric English Comments
Specific Gravity 1.34 g/cc
1.34 g/cc
ASTM D792
Linear Mold Shrinkage 0.003 - 0.006 cm/cm
0.003 - 0.006 in/in
Melt Flow 27 g/10 min

@Load 2.16 kg,
Temperature 210 °C
27 g/10 min

@Load 4.76 lb,
Temperature 410 °F
ASTM D1238
Mechanical Properties Metric English Comments
Flexural Modulus 2.450 GPa
355.3 ksi
ASTM D790
Izod Impact, Notched 0.330 J/cm
0.618 ft-lb/in
ASTM D256
Thermal Properties Metric English Comments
Melting Point 170 °C
338 °F
ASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 50.0 °C
122 °F
ASTM D648
Processing Properties Metric English Comments
Feed Temperature 175 - 185 °C
347 - 365 °F
Nozzle Temperature 190 - 210 °C
374 - 410 °F
Mold Temperature 25.0 °C
77.0 °F
Back Pressure 0.345 - 0.689 MPa
50.0 - 100 psi
Screw Speed 100 - 200 rpm
100 - 200 rpm