| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.19 g/cc | 1.19 g/cc | ASTM D792 |
| Density | 1.19 g/cc | 0.0430 lb/in³ | ISO 1183 |
| Moisture Absorption | 0.0900 % | 0.0900 % | 23°C / 50% RH; ISO 62 |
| Water Absorption at Saturation | 0.12 % | 0.12 % | ISO 62 |
| Linear Mold Shrinkage, Flow | 0.0040 - 0.0080 cm/cm <br>@Thickness 3.20 mm |
0.0040 - 0.0080 in/in <br>@Thickness 0.126 in |
SABIC Method |
| Linear Mold Shrinkage, Transverse | 0.0040 - 0.0080 cm/cm <br>@Thickness 3.20 mm |
0.0040 - 0.0080 in/in <br>@Thickness 0.126 in |
SABIC Method |
| Melt Flow | 35 g/10 min <br>@Load 1.20 kg,<br> Temperature 300 °C |
35 g/10 min <br>@Load 2.65 lb,<br> Temperature 572 °F |
ASTM D1238 |
| Melt Index of Compound | 33 g/10 min <br>@Load 1.20 kg,<br> Temperature 300 °C |
33 g/10 min <br>@Load 2.65 lb,<br> Temperature 572 °F |
MVR [cm^3/10 min]; ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell L | 90 | 90 | ASTM D785 |
| Tensile Strength at Break | 56.0 MPa | 8120 psi | 50 mm/min; ISO 527 |
| 58.0 MPa | 8410 psi | Type I, 50 mm/min; ASTM D638 | |
| Tensile Strength, Yield | 59.0 MPa | 8560 psi | Type I, 50 mm/min; ASTM D638 |
| 59.0 MPa | 8560 psi | 50 mm/min; ISO 527 | |
| Elongation at Break | 118.6 % | 118.6 % | 50 mm/min; ISO 527 |
| 118.9 % | 118.9 % | Type I, 50 mm/min; ASTM D638 | |
| Elongation at Yield | 5.4 % | 5.4 % | 50 mm/min; ISO 527 |
| 5.7 % | 5.7 % | Type I, 50 mm/min; ASTM D638 | |
| Tensile Modulus | 2.36 GPa | 342 ksi | 50 mm/min; ASTM D638 |
| 2.40 GPa | 348 ksi | 1 mm/min; ISO 527 | |
| Flexural Yield Strength | 92.0 MPa | 13300 psi | 2 mm/min; ISO 178 |
| 99.0 MPa | 14400 psi | 1.3 mm/min, 50 mm span; ASTM D790 | |
| Flexural Modulus | 2.25 GPa | 326 ksi | 2 mm/min; ISO 178 |
| 2.35 GPa | 341 ksi | 1.3 mm/min, 50 mm span; ASTM D790 | |
| Izod Impact, Notched | 7.02 J/cm | 13.2 ft-lb/in | ASTM D256 |
| 2.20 J/cm <br>@Temperature -30.0 °C |
4.12 ft-lb/in <br>@Temperature -22.0 °F |
ASTM D256 | |
| Izod Impact, Notched (ISO) | 60.0 kJ/m² | 28.6 ft-lb/in² | 80*10*3; ISO 180/1A |
| 30.0 kJ/m² <br>@Temperature -30.0 °C |
14.3 ft-lb/in² <br>@Temperature -22.0 °F |
80*10*3; ISO 180/1A | |
| Izod Impact, Unnotched (ISO) | NB | NB | 80*10*3; ISO 180/1U |
| NB <br>@Temperature -30.0 °C |
NB <br>@Temperature -22.0 °F |
80*10*3; ISO 180/1U | |
| Charpy Impact Unnotched | NB | NB | Edgew 80*10*3 sp=62mm; ISO 179/1eU |
| NB <br>@Temperature -30.0 °C |
NB <br>@Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eU | |
| Charpy Impact, Notched | 6.50 J/cm² | 30.9 ft-lb/in² | Edgew 80*10*3 sp=62mm; ISO 179/1eA |
| 4.00 J/cm² <br>@Temperature -30.0 °C |
19.0 ft-lb/in² <br>@Temperature -22.0 °F |
Edgew 80*10*3 sp=62mm; ISO 179/1eA | |
| Dart Drop, Total Energy | 79.0 J <br>@Temperature 23.0 °C |
58.3 ft-lb <br>@Temperature 73.4 °F |
ASTM D3763 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 65.0 µm/m-°C <br>@Temperature -40.0 - 95.0 °C |
36.1 µin/in-°F <br>@Temperature -40.0 - 203 °F |
ASTM E 831 |
| 65.0 µm/m-°C <br>@Temperature 23.0 - 80.0 °C |
36.1 µin/in-°F <br>@Temperature 73.4 - 176 °F |
ISO 11359-2 | |
| CTE, linear, Transverse to Flow | 74.0 µm/m-°C <br>@Temperature -40.0 - 95.0 °C |
41.1 µin/in-°F <br>@Temperature -40.0 - 203 °F |
ASTM E 831 |
| 74.0 µm/m-°C <br>@Temperature 23.0 - 80.0 °C |
41.1 µin/in-°F <br>@Temperature 73.4 - 176 °F |
ISO 11359-2 | |
| Deflection Temperature at 1.8 MPa (264 psi) | 117 °C | 243 °F | Flatw 80*10*4 sp=64mm; ISO 75/Af |
| 120 °C <br>@Thickness 3.20 mm |
248 °F <br>@Thickness 0.126 in |
unannealed; ASTM D648 | |
| Vicat Softening Point | 137 °C | 279 °F | Rate B/50; ISO 306 |
| 138 °C | 280 °F | Rate A/50; ASTM D1525 | |
| 140 °C | 284 °F | Rate B/120; ISO 306 | |
| UL RTI, Electrical | 130 °C | 266 °F | UL 746B |
| UL RTI, Mechanical without Impact | 130 °C | 266 °F | UL 746B |
| Flammability, UL94 | HB <br>@Thickness 1.50 mm |
HB <br>@Thickness 0.0591 in |
UL 94 |
| Glow Wire Test | 825 °C | 1520 °F | IEC 60695-2-13 |
| 850 °C | 1560 °F | IEC 60695-2-13 | |
| 960 °C <br>@Thickness 3.00 mm |
1760 °F <br>@Thickness 0.118 in |
IEC 60695-2-12 |
| Optical Properties | Metric | English | Comments |
|---|---|---|---|
| Haze | 3.0 % <br>@Thickness 2.54 mm |
3.0 % <br>@Thickness 0.100 in |
ASTM D1003 |
| Transmission, Visible | 82 % | 82 % | 2.54 mm; ASTM D1003 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | >= 1.00e+15 ohm-cm | >= 1.00e+15 ohm-cm | ASTM D257 |
| Surface Resistance | >= 1.00e+15 ohm | >= 1.00e+15 ohm | ASTM D257 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Ball Pressure Test, 125°C +/- 2°C | PASS | IEC 60695-10-2 |