Category Polymer , Thermoset , Diallyl Phthalate (DAP) , Diallyl Phthalate (DAP) Molding Compound, Short Glass Fiber Filled , Filled/Reinforced Thermoset
Manufacturer Raschig Group
Trade Name
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Raschig Group 5562 DAP.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Glass-fiber reinforced diallyl phthalate molding compound. Good mechanical strength together with retention of high electrical isolation properties under hot humid conditions, exceptional dimensional stability even under severe environmental conditions. This product meets the allowed upper limits for heavy metals and PCAs and also conforms to the requirements of the EU directives 2002/95 (RoHS), 2002/96 (WEEE) and 2006/122 (PFOS)Processing: Injection and transfer moldingApplications: Connectors, Bobbins, Potentiometers, switchesInformation provided by the Raschig Group
Physical Properties Metric English Comments
Specific Gravity 1.80 - 2.00 g/cc
1.80 - 2.00 g/cc
ISO 1183
Apparent Bulk Density 0.750 - 0.900 g/cc
0.0271 - 0.0325 lb/in³
ISO 60
Water Absorption <= 0.20 %
<br>@Temperature 23.0 °C,<br> Time 86400 sec
<= 0.20 %
<br>@Temperature 73.4 °F,<br> Time 24.0 hour
ISO 62
Linear Mold Shrinkage 0.0015 - 0.0045 cm/cm
0.0015 - 0.0045 in/in
Injection; ISO 2577
Mechanical Properties Metric English Comments
Tensile Strength, Yield 80.0 - 90.0 MPa
11600 - 13100 psi
Injection; ISO 527
Modulus of Elasticity 10.0 - 14.0 GPa
1450 - 2030 ksi
Injection; ISO 527
Flexural Strength 120 - 160 MPa
17400 - 23200 psi
Injection; ISO 178
Flexural Modulus 11.0 - 14.0 GPa
1600 - 2030 ksi
Injection; ISO 178
Compressive Strength 150 - 200 MPa
21800 - 29000 psi
ISO 604
Charpy Impact Unnotched 0.700 - 1.00 J/cm²
<br>@Temperature 23.0 °C
3.33 - 4.76 ft-lb/in²
<br>@Temperature 73.4 °F
Injection; ISO 179/ 1eU
Charpy Impact, Notched 0.350 - 0.450 J/cm²
<br>@Temperature 23.0 °C
1.67 - 2.14 ft-lb/in²
<br>@Temperature 73.4 °F
Injection; ISO 179/ 1eA
Thermal Properties Metric English Comments
CTE, linear 5.00 - 10.0 µm/m-°C
<br>@Temperature 50.0 - 100 °C
2.78 - 5.56 µin/in-°F
<br>@Temperature 122 - 212 °F
ISO 11359-2
Thermal Conductivity 0.900 - 1.10 W/m-K
6.25 - 7.63 BTU-in/hr-ft²-°F
ASTM E1461
Deflection Temperature at 1.8 MPa (264 psi) >= 200 °C
>= 392 °F
Injection; ISO 75-A
Deflection Temperature at 8.0 MPa 130 - 150 °C
266 - 302 °F
Injection; ISO 75-C
Flammability, UL94 V-0
<br>@Thickness 0.700 mm
V-0
<br>@Thickness 0.0276 in
Shrinkage <= 0.050 %
<br>@Temperature 110 °C,<br> Time 605000 sec
<= 0.050 %
<br>@Temperature 230 °F,<br> Time 168 hour
Post shrinkage; ISO 2577
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+14 - 1.00e+15 ohm-cm
1.00e+14 - 1.00e+15 ohm-cm
IEC 60093
Surface Resistance 1.00e+14 - 1.00e+15 ohm
1.00e+14 - 1.00e+15 ohm
IEC 60093
Dielectric Constant 4.0 - 4.5
<br>@Frequency 1.00e+6 Hz
4.0 - 4.5
<br>@Frequency 1.00e+6 Hz
IEC 60250
4.5 - 5.0
<br>@Frequency 100 Hz
4.5 - 5.0
<br>@Frequency 100 Hz
IEC 60250
Dielectric Strength 15.0 - 20.0 kV/mm
381 - 508 kV/in
IEC 60243-1
Dissipation Factor 0.010 - 0.030
<br>@Frequency 100 Hz
0.010 - 0.030
<br>@Frequency 100 Hz
IEC 60250
0.010 - 0.030
<br>@Frequency 1.00e+6 Hz
0.010 - 0.030
<br>@Frequency 1.00e+6 Hz
IEC 60250
Comparative Tracking Index >= 500 V
>= 500 V
CTI; IEC 60112
Processing Properties Metric English Comments
Shelf Life 6.00 Month
<br>@Temperature 15.0 - 25.0 °C
6.00 Month
<br>@Temperature 59.0 - 77.0 °F
Descriptive Properties Value Comments
Arc Resistance 4 Stufe
ASTM D495
Glow wire flammability test 960/0.6
DIN EN 60695-2-11
Glow wire ignitability test 875/0.6
DIN EN 60695-2-13
Water Absorption <15 mg
ISO 62; 24h / 23°C
Copyright © lookpolymers.com All Rights Reserved