| Category | Metal , Nonferrous Metal , Nickel Alloy , Superalloy |
| Manufacturer | Haynes International, Inc. |
| Trade Name | |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Haynes 214® alloy, 20% cold reduction, 925°C for 5 minutes.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 8.05 g/cc | 0.291 lb/in³ | at RT |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Brinell | 262 | 262 | Converted from Rockwell C hardness. |
| Hardness, Knoop | 284 | 284 | Converted from Rockwell C hardness. |
| Hardness, Rockwell C | 25.1 | 25.1 | |
| Hardness, Vickers | 270 | 270 | Converted from Rockwell C hardness. |
| Tensile Strength, Ultimate | 1030 MPa | 149000 psi | |
| Tensile Strength, Yield | 610 MPa <br>@Strain 0.200 % |
88500 psi <br>@Strain 0.200 % |
|
| Elongation at Break | 34.6 % | 34.6 % | in 50.8 mm |
| Modulus of Elasticity | 218 GPa | 31600 ksi | RT |
| 137 GPa <br>@Temperature 1000 °C |
19900 ksi <br>@Temperature 1830 °F |
||
| 151 GPa <br>@Temperature 900 °C |
21900 ksi <br>@Temperature 1650 °F |
||
| 162 GPa <br>@Temperature 800 °C |
23500 ksi <br>@Temperature 1470 °F |
||
| 170 GPa <br>@Temperature 700 °C |
24700 ksi <br>@Temperature 1290 °F |
||
| 177 GPa <br>@Temperature 600 °C |
25700 ksi <br>@Temperature 1110 °F |
||
| 184 GPa <br>@Temperature 500 °C |
26700 ksi <br>@Temperature 932 °F |
||
| 190 GPa <br>@Temperature 400 °C |
27600 ksi <br>@Temperature 752 °F |
||
| 199 GPa <br>@Temperature 300 °C |
28900 ksi <br>@Temperature 572 °F |
||
| 204 GPa <br>@Temperature 200 °C |
29600 ksi <br>@Temperature 392 °F |
||
| 210 GPa <br>@Temperature 100 °C |
30500 ksi <br>@Temperature 212 °F |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 13.3 µm/m-°C <br>@Temperature 25.0 - 200 °C |
7.39 µin/in-°F <br>@Temperature 77.0 - 392 °F |
|
| 13.6 µm/m-°C <br>@Temperature 25.0 - 300 °C |
7.56 µin/in-°F <br>@Temperature 77.0 - 572 °F |
||
| 14.1 µm/m-°C <br>@Temperature 25.0 - 400 °C |
7.83 µin/in-°F <br>@Temperature 77.0 - 752 °F |
||
| 14.6 µm/m-°C <br>@Temperature 25.0 - 500 °C |
8.11 µin/in-°F <br>@Temperature 77.0 - 932 °F |
||
| 15.2 µm/m-°C <br>@Temperature 25.0 - 600 °C |
8.44 µin/in-°F <br>@Temperature 77.0 - 1110 °F |
||
| 15.8 µm/m-°C <br>@Temperature 25.0 - 700 °C |
8.78 µin/in-°F <br>@Temperature 77.0 - 1290 °F |
||
| 16.6 µm/m-°C <br>@Temperature 25.0 - 800 °C |
9.22 µin/in-°F <br>@Temperature 77.0 - 1470 °F |
||
| 17.6 µm/m-°C <br>@Temperature 25.0 - 900 °C |
9.78 µin/in-°F <br>@Temperature 77.0 - 1650 °F |
||
| 18.6 µm/m-°C <br>@Temperature 25.0 - 1000 °C |
10.3 µin/in-°F <br>@Temperature 77.0 - 1830 °F |
||
| Specific Heat Capacity | 0.452 J/g-°C | 0.108 BTU/lb-°F | RT |
| 0.470 J/g-°C <br>@Temperature 100 °C |
0.112 BTU/lb-°F <br>@Temperature 212 °F |
||
| 0.493 J/g-°C <br>@Temperature 200 °C |
0.118 BTU/lb-°F <br>@Temperature 392 °F |
||
| 0.515 J/g-°C <br>@Temperature 300 °C |
0.123 BTU/lb-°F <br>@Temperature 572 °F |
||
| 0.538 J/g-°C <br>@Temperature 400 °C |
0.129 BTU/lb-°F <br>@Temperature 752 °F |
||
| 0.561 J/g-°C <br>@Temperature 500 °C |
0.134 BTU/lb-°F <br>@Temperature 932 °F |
||
| 0.611 J/g-°C <br>@Temperature 600 °C |
0.146 BTU/lb-°F <br>@Temperature 1110 °F |
||
| 0.668 J/g-°C <br>@Temperature 700 °C |
0.160 BTU/lb-°F <br>@Temperature 1290 °F |
||
| 0.705 J/g-°C <br>@Temperature 800 °C |
0.168 BTU/lb-°F <br>@Temperature 1470 °F |
||
| 0.728 J/g-°C <br>@Temperature 900 °C |
0.174 BTU/lb-°F <br>@Temperature 1650 °F |
||
| 0.742 J/g-°C <br>@Temperature 1000 °C |
0.177 BTU/lb-°F <br>@Temperature 1830 °F |
||
| 0.749 J/g-°C <br>@Temperature 1100 °C |
0.179 BTU/lb-°F <br>@Temperature 2010 °F |
||
| 0.753 J/g-°C <br>@Temperature 1200 °C |
0.180 BTU/lb-°F <br>@Temperature 2190 °F |
||
| Thermal Conductivity | 12.0 W/m-K | 83.3 BTU-in/hr-ft²-°F | RT |
| 12.8 W/m-K <br>@Temperature 100 °C |
88.8 BTU-in/hr-ft²-°F <br>@Temperature 212 °F |
||
| 14.2 W/m-K <br>@Temperature 200 °C |
98.5 BTU-in/hr-ft²-°F <br>@Temperature 392 °F |
||
| 15.9 W/m-K <br>@Temperature 300 °C |
110 BTU-in/hr-ft²-°F <br>@Temperature 572 °F |
||
| 18.4 W/m-K <br>@Temperature 400 °C |
128 BTU-in/hr-ft²-°F <br>@Temperature 752 °F |
||
| 21.1 W/m-K <br>@Temperature 500 °C |
146 BTU-in/hr-ft²-°F <br>@Temperature 932 °F |
||
| 23.9 W/m-K <br>@Temperature 600 °C |
166 BTU-in/hr-ft²-°F <br>@Temperature 1110 °F |
||
| 26.9 W/m-K <br>@Temperature 700 °C |
187 BTU-in/hr-ft²-°F <br>@Temperature 1290 °F |
||
| 29.7 W/m-K <br>@Temperature 800 °C |
206 BTU-in/hr-ft²-°F <br>@Temperature 1470 °F |
||
| 31.4 W/m-K <br>@Temperature 900 °C |
218 BTU-in/hr-ft²-°F <br>@Temperature 1650 °F |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Electrical Resistivity | 0.0001359 ohm-cm | 0.0001359 ohm-cm | RT |
| 0.0001209 ohm-cm <br>@Temperature 1050 °C |
0.0001209 ohm-cm <br>@Temperature 1920 °F |
||
| 0.000121 ohm-cm <br>@Temperature 1100 °C |
0.000121 ohm-cm <br>@Temperature 2010 °F |
||
| 0.0001216 ohm-cm <br>@Temperature 1000 °C |
0.0001216 ohm-cm <br>@Temperature 1830 °F |
||
| 0.0001219 ohm-cm <br>@Temperature 1150 °C |
0.0001219 ohm-cm <br>@Temperature 2100 °F |
||
| 0.0001229 ohm-cm <br>@Temperature 1200 °C |
0.0001229 ohm-cm <br>@Temperature 2190 °F |
||
| 0.0001249 ohm-cm <br>@Temperature 900 °C |
0.0001249 ohm-cm <br>@Temperature 1650 °F |
||
| 0.0001292 ohm-cm <br>@Temperature 800 °C |
0.0001292 ohm-cm <br>@Temperature 1470 °F |
||
| 0.0001337 ohm-cm <br>@Temperature 700 °C |
0.0001337 ohm-cm <br>@Temperature 1290 °F |
||
| 0.0001368 ohm-cm <br>@Temperature 600 °C |
0.0001368 ohm-cm <br>@Temperature 1110 °F |
||
| 0.0001369 ohm-cm <br>@Temperature 100 °C |
0.0001369 ohm-cm <br>@Temperature 212 °F |
||
| 0.0001369 ohm-cm <br>@Temperature 200 °C |
0.0001369 ohm-cm <br>@Temperature 392 °F |
||
| 0.0001369 ohm-cm <br>@Temperature 300 °C |
0.0001369 ohm-cm <br>@Temperature 572 °F |
||
| 0.0001369 ohm-cm <br>@Temperature 300 °C |
0.0001369 ohm-cm <br>@Temperature 572 °F |
||
| 0.0001377 ohm-cm <br>@Temperature 400 °C |
0.0001377 ohm-cm <br>@Temperature 752 °F |
||
| 0.0001379 ohm-cm <br>@Temperature 500 °C |
0.0001379 ohm-cm <br>@Temperature 932 °F |